Method for avoiding stress marks on surface of double-shot molding INS part
By optimizing the thickness of PC material and injection molding process, combined with the use of PC and ABS materials, the problem of surface stress marks of two-color injection molded INS diaphragms is solved, achieving higher appearance quality and durability.
Patent Information
- Application Number
- CN202411196997.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The sudden change in the wall thickness of the two-color injection molded INS diaphragm at the junction of the primary and dielectric materials causes overall shrinkage, resulting in stress marks, affecting the appearance quality of the product.
By optimizing the thickness of the mono-injection material and di-injection material, the PC material covers the entire surface of the part and performs a 1:30 transition optimization at the junction of the mono-injection and di-injection to reduce injection molding stress, and control injection molding with the use of PC and ABS materials. Process parameters and mold structure, real-time monitoring of the injection molding process, annealing and surface treatment to reduce stress traces.
It effectively avoids the surface stress marks of the two-color INS diaphragm, and improves the appearance quality and durability of the product.
Smart Images

Figure CN118990925A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of two-color injection molded INS diaphragms, and in particular to a method for avoiding stress marks on the surface of two-color injection molded INS parts. Background Art
[0002] Two-color injection molding technology can achieve the fusion of two different colors or materials, making the INS diaphragm have richer colors and layers, and improving the aesthetics of the product. Two-color injection INS diaphragms usually contain multi-layer structures, such as the outer light-transmitting plastic plate, INS diaphragm, inner light-transmitting plastic plate and spray paint light-shielding layer, etc. These structures are closely combined together through precise injection molding technology. The two-color injection molding process can select plastic materials with different properties, such as a combination of hard plastic and soft plastic, thereby improving the physical properties of parts such as wear resistance and impact resistance.
[0003] After searching, the patent with application number CN202111278017.X discloses an automotive interior and exterior trim with a two-color injection molded intermediate INS diaphragm, including an outer light-transmitting plastic plate, an INS diaphragm, an inner light-transmitting plastic plate and a spray-painted light-shielding layer arranged from top to bottom, the INS diaphragm includes a PMMA acrylic layer, an ink-printed light-transmitting layer and an ABS transparent substrate layer composited from top to bottom, one side of the bottom surface of the INS diaphragm is molded as a whole with the inner plastic plate by injection molding, and one side of the top surface of the INS diaphragm is molded as a whole with the outer plastic plate by two-color injection molding, and the spray-painted light-shielding layer is processed with a light-transmitting pattern for light to pass through. The surface processed light-transmitting pattern of this invention has high precision, and the specific shape of the light-transmitting pattern will not be affected by deformation during the product molding process, and the inner and outer sides of the INS diaphragm are respectively provided with an inner light-transmitting plastic plate and an outer light-transmitting plastic plate, which has good weather resistance.
[0004] In the current two-shot injection molding process of INS diaphragms, the wall thickness of the second shot material at the junction of the first shot material and the second shot material suddenly changes, such as Figure 1 As shown in the figure, after two-shot injection molding, the INS diaphragm undergoes overall secondary shrinkage, and the junction of the two colors is affected by the shrinkage of the two-shot product, resulting in stress marks on the surface of the two-color INS diaphragm. Therefore, we need to propose a method to avoid stress marks on the surface of two-shot injection molded INS parts. Summary of the invention
[0005] The object of the present invention is to provide a method for avoiding stress marks on the surface of two-color injection molded INS parts. By optimizing the thickness of the first shot material and the second shot material, the PC material covers the entire surface of the part and is compounded with the INS diaphragm. At the junction of the first shot and the second shot, the thickness of the PC material is optimized by a 1:30 transition, thereby reducing the injection stress. The stress mark phenomenon on the surface of the two-color INS diaphragm can be effectively avoided. The obtained INS diaphragm product has good appearance quality, thereby solving the problems raised in the above-mentioned background technology.
[0006] To achieve the above object, the present invention provides the following technical solution: a method for avoiding stress marks on the surface of two-color injection molded INS parts, comprising the following steps:
[0007] S1. Material preparation: Select PC materials and PC+ABS materials with stable performance, and dry the PC materials to remove moisture from them to prevent bubbles and stress from being generated during the injection molding process;
[0008] S2. Product preparation: According to the design requirements, select INS parts with suitable size, shape and function, and spread the PC material on the surface of the INS parts;
[0009] S3. PC material thickness optimization: The thickness of PC material is designed to be 2.5-3mm, and at the junction of the first shot and the second shot, the thickness of PC material is optimized by 1:30 transition, so that the PC thickness at the edge of INS diaphragm is 1.8-2.3mm;
[0010] S4. PC+ABS material thickness design: The thickness of PC+ABS material gradually transitions from 0.2mm at the junction of the first shot and the second shot to 1.2-1.5mm at the edge;
[0011] S5. Injection molding process control and optimization: According to the characteristics of PC material and PC+ABS material and the mold structure, set the appropriate injection molding temperature, injection molding pressure, injection molding speed and holding time, and monitor the injection molding parameters in real time during the injection molding process;
[0012] S6. Post-processing: annealing, surface treatment and quality inspection of the injection molded INS diaphragm.
[0013] Preferably, in step S1, when the PC material is dried, the drying temperature is controlled between 80-100°C, and the drying time of the PC material is not less than 4 hours. The higher the humidity and thickness of the PC material, the longer the drying time. The humidity of the PC material after drying is less than 0.02%.
[0014] Preferably, in step S2, after the PC material and the INS diaphragm are compounded, a reasonable mold structure needs to be designed and selected, and the mold structure includes a runner, a gate and an exhaust system, so that the melt of the PC material and the PC+ABS material can fill the mold cavity evenly and quickly, and ensure that the mold temperature is evenly distributed to avoid stress problems caused by local overheating or overcooling.
[0015] Preferably, in step S3, the PC material includes a main body portion compounded at a middle position of the INS diaphragm and an edge portion compounded at an edge position of the INS diaphragm;
[0016] The thickness of the main body is 2.5-3 mm, which is used to provide sufficient strength and stability;
[0017] The thickness of the edge portion is 1.8 to 2.3 mm, ensuring the strength and aesthetics of the edge of the INS diaphragm.
[0018] Preferably, in step S4, the PC material adopts a smooth transition at a ratio of 1:30, that is, transitioning from the 3mm area of the first shot to the 0.2mm area of the second shot. The PC+ABS material is used as the second shot material, and the thickness of the second shot material gradually transitions from 0.2mm at the junction to 1.2-1.5mm at the edge, which helps the PC material and PC+ABS material to be well combined at the junction of the first shot and the second shot and reduces stress marks.
[0019] Preferably, in step S5, the injection molding temperature of the PC material is controlled between 250-300°C, and the injection molding temperature of the PC+ABS material is controlled between 240-280°C;
[0020] Adjust the injection pressure value so that the melt of PC material and PC+ABS material can fully fill the mold cavity, and gradually increase the injection pressure during the injection process until the plastic material melt is stably discharged;
[0021] Adjust the injection speed, slow down the injection speed when the plastic material melt passes through the gate, use high-speed injection during the mold filling process, and slow down the speed at the end of mold filling;
[0022] The INS diaphragm is fully solidified and shrinkage deformation is reduced through the pressure holding treatment. The mold applies a stable pressure holding pressure to the plastic material to prevent the INS diaphragm from sinking or changing in size.
[0023] Preferably, when monitoring the injection molding parameters in real time, the monitoring equipment on the injection molding machine is used to observe the parameter changes of injection pressure, injection temperature, and injection speed during the injection molding process in real time, and the exhaust condition of the mold is checked regularly to ensure that the air path is unobstructed and to avoid the generation of bubbles and stress marks; when any abnormal situation is found during the injection molding process, the machine is stopped immediately to check the injection molding parameters.
[0024] Preferably, in step S6, annealing treatment is performed to release the residual stress inside the INS diaphragm through heating and cooling processes to reduce stress marks and deformation. The specific process is as follows:
[0025] Place the injection molded INS diaphragm in an annealing furnace, heat it to a temperature lower than the glass transition temperature of PC material and PC+ABS material, and keep it for a period of time to release the stress inside the INS diaphragm, and then slowly cool it to room temperature to avoid thermal stress caused by rapid cooling.
[0026] Preferably, the surface treatment comprises:
[0027] Grinding and polishing: Use grinding tools and polishing agents to grind and polish the sides of the INS diaphragm to remove burrs, flash and surface defects generated during the injection molding process;
[0028] Cleaning: Use a detergent to clean the surface of the INS diaphragm to remove oil, dust and other impurities to ensure that the surface of the INS diaphragm is clean and free of defects.
[0029] Preferably, quality testing includes:
[0030] Appearance inspection: Use naked eyes to inspect the appearance of the INS diaphragm to check whether there are obvious defects on the INS diaphragm, including cracks, bubbles, dents, uneven colors and stress marks;
[0031] Dimension measurement: Use precision measuring tools to measure the dimensions of INS diaphragms through sampling inspection to see if they meet the design requirements and tolerance requirements, and evaluate the dimensional consistency of INS diaphragms in the same batch;
[0032] Material performance test: Test the melting point, strength, hardness, and toughness of the INS diaphragm, and evaluate the durability and reliability of the INS diaphragm.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The present invention optimizes the thickness of the first shot material and the second shot material, the PC material covers the entire surface of the part and is compounded with the INS diaphragm, and the thickness of the PC material is transitionally optimized to 1:30 at the junction of the first shot and the second shot, thereby reducing the injection stress and effectively avoiding the stress mark phenomenon on the surface of the two-color INS diaphragm. The obtained INS diaphragm product has good appearance quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is a cross-sectional view of an INS diaphragm of the prior art;
[0036] Figure 2 A cross-sectional view of the INS diaphragm prepared by the present invention;
[0037] Figure 3 It is a flowchart of the present invention.
[0038] In the figure: 1. INS diaphragm; 2. PC material; 3. PC+ABS material; 4. Light guide board; 5. Shading substrate. DETAILED DESCRIPTION
[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] See also Figure 2-3 The present invention provides a technical solution: a method for avoiding stress marks on the surface of a two-color injection molded INS part, comprising the following steps:
[0041] S1. Material preparation: Select PC material 2 and PC+ABS material 3 with stable performance, and dry PC material 2 to remove moisture in PC material 2 to prevent bubbles and stress from being generated during the injection molding process;
[0042] In step S1, when the PC material 2 is dried, the drying temperature is controlled between 80-100°C, and the drying time of the PC material 2 is not less than 4 hours. The higher the humidity and thickness of the PC material 2, the longer the drying time. The humidity of the PC material 2 after drying is less than 0.02%.
[0043] S2. Product preparation: According to the design requirements, select INS parts with suitable size, shape and function, and spread the PC material on the surface of the INS parts;
[0044] The INS membrane comprises a light guide plate 4, a light shielding substrate 5 is installed on one side of the light guide plate 4, an INS membrane 1 is arranged on the other side of the light guide plate 4, and PC material 2 and PC+ABS material 3 molded by two-color injection molding process are attached to the INS membrane 1.
[0045] During the product design phase, special attention is paid to areas where stress marks may occur. For example, sharp corners and sharp thickness changes are avoided to reduce stress concentrations.
[0046] In step S2, after the PC material 2 is compounded with the INS diaphragm, a reasonable mold structure needs to be designed and selected. The mold structure includes a runner, a gate and an exhaust system, so that the melt of the PC material 2 and the PC+ABS material 3 can fill the mold cavity evenly and quickly, and ensure that the mold temperature is evenly distributed to avoid stress problems caused by local overheating or overcooling.
[0047] Ensure that the gate size is appropriate and evenly distributed to avoid insufficient filling due to too small or too few gates. Add cold wells or overflow slots to improve the filling effect.
[0048] Design a balanced mold temperature control system to ensure balanced mold temperature and avoid excessive local temperature. Set up water wells in the mold or use 3D printed conformal water channels to solve the problem of uneven mold temperature.
[0049] The plastic injection mold runner and cavity should be designed with a good exhaust system to reduce the stress and pressure in the mold cavity. More exhaust holes should be opened around the mold to ensure that the gas in the mold cavity is discharged smoothly during injection;
[0050] Ensure that the moving parts (such as lifters, sliders, etc.) are tightly fitted to avoid looseness that may cause the mold temperature to rise. Optimize the water channel configuration to ensure a good cooling effect.
[0051] S3. PC material 2 thickness optimization: The thickness of PC material 2 is designed to be 2.5-3mm, and at the junction of the first shot and the second shot, the thickness of PC material 2 is optimized by 1:30, so that the PC thickness at the edge of the INS diaphragm is 1.8-2.3mm;
[0052] In step S3, the PC material 2 includes a main body portion compounded at the middle position of the INS diaphragm and an edge portion compounded at the edge position of the INS diaphragm;
[0053] The thickness of the main body is 2.5-3 mm, which is used to provide sufficient strength and stability;
[0054] The thickness of the edge portion is 1.8-2.3 mm, ensuring the strength and aesthetics of the edge of the INS diaphragm. The thickness of the edge portion should not be too thin to prevent shrinkage deformation and stress marks during the injection molding process.
[0055] Reasonable exhaust grooves can be designed in the mold to ensure that the gas can be discharged smoothly during the injection molding process and reduce the generation of bubbles and stress marks.
[0056] S4. Thickness design of PC+ABS material 3: The thickness of PC+ABS material 3 gradually transitions from 0.2mm at the junction of the first shot and the second shot to 1.2-1.5mm at the edge to reduce stress concentration;
[0057] In step S4, PC material 2 adopts a smooth transition at a ratio of 1:30, that is, transitioning from the 3mm area of the first shot to the 0.2mm area of the second shot. PC+ABS material 3 is used as the second shot material, and the thickness of the second shot material gradually transitions from 0.2mm at the junction to 1.2-1.5mm at the edge, which helps PC material 2 and PC+ABS material 3 to be well combined at the junction of the first shot and the second shot, and reduces stress marks.
[0058] S5. Injection molding process control and optimization: according to the characteristics of PC material 2 and PC+ABS material 3 and the mold structure, set the appropriate injection molding temperature, injection molding pressure, injection molding speed and holding time, and monitor the injection molding parameters in real time during the injection molding process;
[0059] In step S5, the injection molding temperature of PC material 2 is controlled between 250-300°C, and the injection molding temperature of PC+ABS material 3 is controlled between 240-280°C;
[0060] Adjust the injection pressure value so that the melt of PC material 2 and PC+ABS material 3 fully fills the mold cavity, and gradually increase the injection pressure during the injection process until the plastic material melt is stably discharged;
[0061] Adjust the injection speed, slow down the injection speed when the plastic material melt passes through the gate, use high-speed injection during the mold filling process, and slow down the speed at the end of mold filling;
[0062] The INS diaphragm is fully solidified and shrinkage deformation is reduced through the pressure holding treatment. The mold applies a stable pressure holding pressure to the plastic material to prevent the INS diaphragm from sinking or changing in size.
[0063] Reasonably set the holding pressure and time to avoid stress marks caused by too high or too low holding pressure, and reduce the injection pressure to reduce stress during the filling process;
[0064] Appropriately increase the material temperature, back pressure and screw speed. If necessary, use electric heating rods or open water channels to run high-temperature hot oil to locally heat the mold to improve stress marks.
[0065] When monitoring injection molding parameters in real time, use the monitoring equipment on the injection molding machine to observe the changes in injection pressure, injection temperature, and injection speed parameters during the injection molding process in real time, and regularly check the exhaust of the mold to ensure that the air path is unobstructed and avoid bubbles and stress marks. When any abnormal situation is found during the injection molding process, stop the machine immediately to check the injection molding parameters.
[0066] Monitor the opening and closing status of the mold in real time to ensure that the mold is opened and closed at the right time;
[0067] Check whether the mold is damaged or abnormal, such as broken ejector pins, fallen inserts, etc., to prevent further damage to the mold;
[0068] Monitor the cleanliness and lubrication of the mold to ensure the normal operation of the mold;
[0069] Real-time monitoring of various parameters of the injection molding machine, such as pressure, temperature, speed, etc., to ensure that these parameters fluctuate within the set range;
[0070] Monitor the clamping force during the injection molding process to ensure that the mold has sufficient clamping force during the injection molding process to prevent the mold from being stretched open;
[0071] Monitor the appearance quality of injection molded products through visual inspection and other technical means, such as burrs, missing materials, deformation and other problems;
[0072] Monitor the dimensional accuracy of products to ensure that they meet design requirements.
[0073] The above monitoring process can be implemented using mold monitors, sensor technology, or machine vision technology.
[0074] S6. Post-processing: annealing, surface treatment and quality inspection of the injection molded INS diaphragm.
[0075] In step S6, annealing treatment: through the heating and cooling process, the residual stress inside the INS diaphragm is released to reduce stress marks and deformation. The specific process is as follows:
[0076] The injection molded INS diaphragm is placed in an annealing furnace and heated to a temperature lower than the glass transition temperature of PC material 2 and PC+ABS material 3, and maintained for a period of time to release the stress inside the INS diaphragm, and then slowly cooled to room temperature to avoid thermal stress caused by rapid cooling.
[0077] Surface treatment includes:
[0078] Grinding and polishing: Use grinding tools and polishing agents to grind and polish the sides of the INS diaphragm to remove burrs, flash and surface defects generated during the injection molding process;
[0079] Cleaning: Use a detergent to clean the surface of the INS diaphragm to remove oil, dust and other impurities to ensure that the surface of the INS diaphragm is clean and free of defects.
[0080] Quality testing includes:
[0081] Appearance inspection: Use naked eyes to inspect the appearance of the INS diaphragm to check whether there are obvious defects on the INS diaphragm, including cracks, bubbles, dents, uneven colors and stress marks;
[0082] Dimension measurement: Use precision measuring tools to measure the dimensions of INS diaphragms through sampling inspection to see if they meet the design requirements and tolerance requirements, and evaluate the dimensional consistency of INS diaphragms in the same batch;
[0083] Material performance test: Test the melting point, strength, hardness, and toughness of the INS diaphragm, and evaluate the durability and reliability of the INS diaphragm.
[0084] Also includes functional tests:
[0085] Pressure testing: Pressure testing is performed on parts that need to withstand pressure to verify their performance under pressure, which helps to evaluate the sealing, pressure resistance and structural strength of the parts;
[0086] Fluid testing: Fluid testing is performed on parts that need to contact fluid to verify their performance in the fluid environment, which helps to evaluate the corrosion resistance, sealing, fluid resistance and other characteristics of the parts;
[0087] Wear resistance test: Wear resistance test is performed on parts that need to withstand wear to verify their wear resistance during use, which helps to evaluate the service life and reliability of the parts.
[0088] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for avoiding stress marks on the surface of two-color injection molded INS parts, characterized in that: The following steps are involved: S1. Material preparation: Select PC materials and PC+ABS materials with stable performance, and dry the PC materials to remove moisture from them to prevent bubbles and stress from being generated during the injection molding process; S2. Product preparation: According to the design requirements, select INS parts with suitable size, shape and function, and spread the PC material on the surface of the INS parts; S3. PC material thickness optimization: The thickness of PC material is designed to be 2.5-3mm, and at the junction of the first shot and the second shot, the thickness of PC material is optimized by 1:30 transition, so that the PC thickness at the edge of INS diaphragm is 1.8-2.3mm; S4. PC+ABS material thickness design: The thickness of PC+ABS material gradually transitions from 0.2mm at the junction of the first shot and the second shot to 1.2-1.5mm at the edge; S5. Injection molding process control and optimization: According to the characteristics of PC material and PC+ABS material and the mold structure, set the appropriate injection molding temperature, injection molding pressure, injection molding speed and holding time, and monitor the injection molding parameters in real time during the injection molding process; S6. Post-processing: annealing, surface treatment and quality inspection of the injection molded INS diaphragm.
2. A method for avoiding stress marks on the surface of double-color injection molded INS parts according to claim 1, characterized in that: In step S1, when the PC material is dried, the drying temperature is controlled between 80-100°C, and the drying time of the PC material is not less than 4 hours. The higher the humidity and thickness of the PC material, the longer the drying time. The humidity of the PC material after drying is less than 0.02%.
3. A method for avoiding stress marks on the surface of two-color injection molded INS parts according to claim 1, characterized in that: In step S2, after the PC material and the INS diaphragm are compounded, a reasonable mold structure needs to be designed and selected. The mold structure includes runners, gates, and exhaust systems, so that the melt of the PC material and PC+ABS material can fill the mold cavity evenly and quickly, and ensure that the mold temperature is evenly distributed to avoid stress problems caused by local overheating or overcooling.
4. A method for avoiding stress marks on the surface of double-color injection molded INS parts according to claim 1, characterized in that: In step S3, the PC material includes a main body portion compounded at a middle position of the INS diaphragm and an edge portion compounded at an edge position of the INS diaphragm; The thickness of the main body is 2.5-3 mm, which is used to provide sufficient strength and stability; The thickness of the edge portion is 1.8 to 2.3 mm, ensuring the strength and aesthetics of the edge of the INS diaphragm.
5. A method for avoiding stress marks on the surface of double-color injection molded INS parts according to claim 1, characterized in that: In step S4, the PC material adopts a smooth transition at a ratio of 1:30, that is, transitioning from the 3mm area of the first shot to the 0.2mm area of the second shot. The PC+ABS material is used as the second shot material, and the thickness of the second shot material gradually transitions from 0.2mm at the junction to 1.2-1.5mm at the edge, which helps the PC material and PC+ABS material to be well combined at the junction of the first shot and the second shot and reduces stress marks.
6. A method for avoiding stress marks on the surface of double-color injection molded INS parts according to claim 1, characterized in that: In step S5, the injection molding temperature of the PC material is controlled between 250-300°C, and the injection molding temperature of the PC+ABS material is controlled between 240-280°C; Adjust the injection pressure value so that the melt of PC material and PC+ABS material can fully fill the mold cavity, and gradually increase the injection pressure during the injection process until the plastic material melt is stably discharged; Adjust the injection speed, slow down the injection speed when the plastic material melt passes through the gate, use high-speed injection during the mold filling process, and slow down the speed at the end of mold filling; The INS diaphragm is fully solidified and shrinkage deformation is reduced through the pressure holding treatment. The mold applies a stable pressure holding pressure to the plastic material to prevent the INS diaphragm from sinking or changing in size.
7. A method for avoiding stress marks on the surface of double-color injection molded INS parts according to claim 6, characterized in that: When monitoring injection molding parameters in real time, use the monitoring equipment on the injection molding machine to observe the changes in injection pressure, injection temperature, and injection speed parameters during the injection molding process in real time, and regularly check the exhaust of the mold to ensure that the air path is unobstructed and avoid bubbles and stress marks. When any abnormal situation is found during the injection molding process, stop the machine immediately to check the injection molding parameters.
8. A method for avoiding stress marks on the surface of double-color injection molded INS parts according to claim 1, characterized in that: In step S6, annealing treatment: through the heating and cooling process, the residual stress inside the INS diaphragm is released to reduce stress marks and deformation. The specific process is as follows: Place the injection molded INS diaphragm in an annealing furnace, heat it to a temperature lower than the glass transition temperature of PC material and PC+ABS material, and keep it for a period of time to release the stress inside the INS diaphragm, and then slowly cool it to room temperature to avoid thermal stress caused by rapid cooling.
9. A method for avoiding stress marks on the surface of double-color injection molded INS parts according to claim 1, characterized in that: Surface treatment includes: Grinding and polishing: Use grinding tools and polishing agents to grind and polish the sides of the INS diaphragm to remove burrs, flash and surface defects generated during the injection molding process; Cleaning: Use a detergent to clean the surface of the INS diaphragm to remove oil, dust and other impurities to ensure that the surface of the INS diaphragm is clean and free of defects.
10. A method for avoiding stress marks on the surface of double-color injection molded INS parts according to claim 1, characterized in that: Quality testing includes: Appearance inspection: Use naked eyes to inspect the appearance of the INS diaphragm to check whether there are obvious defects on the INS diaphragm, including cracks, bubbles, dents, uneven colors and stress marks; Dimension measurement: Use precision measuring tools to measure the dimensions of INS diaphragms through sampling inspection to see if they meet the design requirements and tolerance requirements, and evaluate the dimensional consistency of INS diaphragms in the same batch; Material performance test: Test the melting point, strength, hardness, and toughness of the INS diaphragm, and evaluate the durability and reliability of the INS diaphragm.
Citation Information
Patent Citations
Self-pushing interlayer injection molding method
CN109531922A
Vehicle-mounted navigation display panel and manufacturing method
CN110667036A
Providing micro-channels in a plastic substrate
EP2653285A1
Two-color molded article and manufacturing method thereof