Preparation method of iron-based multi-element doped Prussian blue positive electrode material with high capacity and long service life

The preparation of iron-based multi-doped Prussian blue cathode material through co-precipitation method solves the problems of high cost and poor cycle stability of the cathode material of sodium ion battery, and achieves electrochemical properties with high specific capacity and long life, which is suitable for large-scale production.

CN118993106APending Publication Date: 2024-11-22SHANDONG HANHANG NEW ENERGY MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411235562.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing sodium ion battery positive electrode materials are costly and have poor cycle stability in large-scale production, resulting in capacity attenuation, especially the high price of cobalt, nickel, copper and other elements in high-entropy Prussian blue materials and the problem of decreasing specific battery capacity.

Method used

The co-precipitation method is used to prepare high capacity, long life iron-based multi-doped Prussian blue positive electrode material. By adding silane coupling agent and additive to solution C, stable silicon-oxygen-carbon bonds and silicon-oxygen-ferrous are formed. bonds increase the reactive sites of sodium ions, and introduce doped elements such as manganese, nickel, copper and zinc to regulate crystal structure and growth kinetics, and improve crystallinity and cyclic stability.

Benefits of technology

The sodium ion battery cathode material with high specific capacity and cycle stability has reduced production costs, improved electrochemical performance, and significantly improved material structural stability and cycle performance, making it suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993106A_ABST
    Figure CN118993106A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a high-capacity long-life iron-based multi-element doped Prussian blue positive electrode material, and belongs to the field of new energy batteries, and the specific scheme comprises the following steps: step 1, dissolving sodium ferrocyanide in deionized water to obtain a solution A; transition metal salt, a complexing agent and an auxiliary agent are dissolved in deionized water to obtain a solution B, and the transition metal salt comprises one or a combination of two of ferric salt and ferrite, one or a combination of more of nickel salt, copper salt and zinc salt, and manganese salt; auxiliary agents and a silane coupling agent are added into deionized water and mixed to be uniform, a solution C is obtained, and the auxiliary agents in the solution B and the solution C both contain carboxylic acid groups; and 2, dropwise adding the solution A and the solution B into the solution C at the same time, stirring, carrying out a co-precipitation reaction, centrifuging, washing, and carrying out vacuum drying to obtain the high-capacity long-life iron-based multi-element doped Prussian blue positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of new energy batteries, relates to the field of sodium ion batteries, and specifically relates to a method for preparing a high-capacity and long-life iron-based multinary doped Prussian blue positive electrode material. Background Art

[0002] The rising price of lithium and the scarcity of lithium resources worldwide have directly led to a significant increase in the manufacturing cost of lithium-ion batteries, hindering their further development. Compared with lithium-ion batteries, sodium-ion batteries not only have the advantages of abundant resources, but also have appropriate redox potential and higher safety. Therefore, for large-scale energy storage devices that require batteries to operate for a long time, sodium-ion batteries have become a viable alternative to lithium-ion batteries.

[0003] At present, potential cathode materials for sodium-ion batteries mainly include Prussian blue analogs (PBAs), layered transition metal oxides, and polyanionic materials. Due to their open skeleton structure, abundant redox active sites, and excellent structural stability, Prussian blue analogs have received great attention as cathode materials for sodium-ion batteries, and they have excellent reversibility and stability. Considering the cost of raw materials during large-scale production, iron-based Prussian blue analogs with high specific capacity (theoretical capacity 170 mAh / g) and low cost are one of the best choices.

[0004] However, due to the crystal defects generated during the synthesis of iron-based Prussian blue and the structural instability during the electrochemical cycle, the reversibility is poor and the capacity decay is fast. In response to the above problems, the invention patent with application publication number CN114805450A discloses a preparation method and application of a high-entropy Prussian blue sodium-ion battery positive electrode material, and prepares a high-entropy Prussian blue sodium-ion battery positive electrode material containing five elements of iron, manganese, cobalt, nickel and copper. Although the high-entropy positive electrode material has a certain improvement in cycle stability, according to the latest market price information, the average price of cobalt is 200,000 to 250,000 yuan / ton, the average price of nickel is about 140,000 yuan / ton, the average price of copper is about 80,000 yuan / ton, and the average price of zinc is 24,000 yuan / ton. On the one hand, due to the high price of cobalt, the types of elements used in this type of high-entropy Prussian blue and the content of nearly one-fifth undoubtedly increase the cost. On the other hand, there are a large number of transition metal elements with single metal active centers such as nickel and copper, and the battery specific capacity is attenuated to a certain extent. Summary of the invention

[0005] In order to prepare a Prussian blue positive electrode material with high specific capacity and excellent cycle performance while ensuring low cost in large-scale production, the present invention provides a method for preparing a high-capacity and long-life iron-based multinary doped Prussian blue positive electrode material.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a high-capacity and long-life iron-based multinary doped Prussian blue positive electrode material comprises the following steps:

[0008] Step 1, dissolving sodium ferrocyanide in deionized water to obtain solution A;

[0009] Dissolving a transition metal salt, a complexing agent and an auxiliary agent in deionized water to obtain a solution B, wherein the transition metal salt comprises one or a combination of two of a ferric salt and a ferrous salt, one or a combination of one or more of a nickel salt, a copper salt and a zinc salt, and a manganese salt;

[0010] Adding an additive and a silane coupling agent to deionized water and mixing well to obtain a solution C, wherein the additives in both the solution B and the solution C contain a carboxylic acid group;

[0011] Step 2: Add solution A and solution B to solution C simultaneously and stir to perform a co-precipitation reaction, centrifuge, wash, and vacuum dry to obtain a long-life iron-based multinary doped Prussian blue positive electrode material;

[0012] The above steps are all carried out under the protection of inert gas.

[0013] Furthermore, the concentration of sodium ferrocyanide in solution A is 0.1-0.4 mol / L.

[0014] Furthermore, in solution B, the iron salt, ferrous salt, nickel salt, copper salt and zinc salt are independently selected from any one or more combinations of chloride, sulfate, nitrate and acetate.

[0015] Furthermore, the ratio of the total molar amount of the transition metal salt to the molar amount of sodium ferrocyanide is 0.5-2.

[0016] Furthermore, in solution B, the total molar amount of iron salt and ferrous salt is 50% to 90% of the total molar amount of transition metal salt, the molar amount of manganese salt is 5% to 40% of the total molar amount of transition metal salt, the molar amount of nickel salt is 0 to 20% of the total molar amount of transition metal salt, the molar amount of copper salt is 0 to 20% of the total molar amount of transition metal salt, and the molar amount of zinc salt is 0 to 20% of the total molar amount of transition metal salt; the molar ratio of the complexing agent to the transition metal cation in the transition metal salt is 1 to 3:1, and the molar ratio of the auxiliary agent to the complexing agent is 1:5 to 30.

[0017] Furthermore, solution C also includes a complexing agent.

[0018] Furthermore, the complexing agent includes one or a combination of sodium citrate, sodium EDTA, and sodium pyrophosphate; the auxiliary agent includes one or a combination of citric acid, tartaric acid, and malic acid; and the silane coupling agent includes one or a combination of vinyl silane coupling agent, amino silane coupling agent, methacryloxy silane coupling agent, epoxy silane coupling agent, and mercapto silane coupling agent.

[0019] Furthermore, in step 2, the dropwise addition rate of solution A and solution B is 1-20 ml / min, the reaction is carried out under mechanical stirring at 300-900 r / min, the reaction temperature is 25° C.-50° C., and the reaction time is 12-24 h.

[0020] Furthermore, in step 2, the vacuum drying temperature is 100-170° C., and the drying time is 12 h to 48 h.

[0021] Furthermore, the mass fraction of the silane coupling agent in the solution C is 1% to 20%, the molar ratio of the complexing agent to the transition metal cation in the transition metal salt is 1 to 6:1, and the molar ratio of the auxiliary agent to the complexing agent is 1:5 to 30.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention uses a coprecipitation method to successfully prepare a sodium ion battery positive electrode material with high specific capacity and cycle stability by adding a silane coupling agent to liquid C. The role of the silane coupling agent in the method is that the silicon bond therein reacts with the carboxylic acid group in the auxiliary agent to form a silicon-oxygen-carbon bond, and on the other hand, it reacts with the surface hydroxyl group of the iron ion to form a stable silicon-oxygen-iron bond, both of which promote the binding of iron ions and carboxylic acid groups on the surface of Prussian blue particles. Due to the high affinity of carboxylic acid ligands with sodium ions, the carboxylic acid groups on the surface of Prussian blue serve as additional reactive active sites for sodium ions, increasing the sodium content. During the battery charge and discharge cycle, sodium ions can be deintercalated from the active sites on the surface, which is beneficial to the improvement of specific capacity. The material is a modified Prussian blue analogue, which is characterized in that manganese is introduced as the main doping component on the basis of iron-based Prussian blue, and is supplemented with a small amount of any one or more of nickel, copper and zinc, which together constitute a complex metal ion system. Compared with single-element iron-based Prussian blue, multi-element doping improves the crystallinity of the characteristic peak of the monoclinic phase (400) crystal plane, thereby reducing structural distortion and improving cycle stability. Its preparation process is simple, the required equipment is not complicated, and the raw material cost is low, making this material have great potential in industrial production. The prepared positive electrode material combines the advantages of high coulomb efficiency of iron-based Prussian blue, high voltage platform of manganese-based Prussian blue, and high cycle stability of nickel-based, copper-based and zinc-based Prussian blue, and has excellent electrochemical performance.

[0024] The present invention adjusts the crystal structure and changes the crystal growth kinetics by multi-element doping, improves the crystallinity of the characteristic peak of the monoclinic phase (400) crystal plane, reduces defects and enhances the stability of the crystal structure. This method improves the problem of low specific capacity of iron-based multi-element doped Prussian blue and improves the initial specific capacity. And by regulating the doping amount of any one or more of the nickel, copper and zinc elements, the production cost of the Prussian blue positive electrode material is greatly reduced; the present invention synthesizes an iron-based Prussian blue with a high sodium content by a coprecipitation method, and controls the amount of manganese and inert elements nickel, copper and zinc, ensuring a long life cycle while avoiding a substantial decrease in specific capacity. The method has the advantages of simplicity, strong controllability, environmental friendliness and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 SEM image of FMNZ-2;

[0026] Figure 2 XRD patterns of FMNZ-1, FMNZ-2, FMNZ-3 and FM-1;

[0027] Figure 3 (400) crystal plane crystallinity diagrams of FMNZ-1, FMNZ-2, FMNZ-3 and FM-1;

[0028] Figure 4 Voltage-specific capacity curve of FMNZ-2;

[0029] Figure 5 Capacity retention diagram of FMNZ-1, FMNZ-2, FMNZ-3 and FM-1;

[0030] Figure 6 Capacity retention diagram of FMNZ-1 and FMNZ-4. DETAILED DESCRIPTION

[0031] The technical solution of the present invention will be clearly and completely described below in conjunction with the drawings and embodiments. Obviously, the described embodiments are only part of the embodiments of the invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0032] Embodiment 1:

[0033] A method for preparing a high-capacity and long-life iron-based multinary doped Prussian blue positive electrode material comprises the following steps:

[0034] Step 1: Weigh 0.15 mol of sodium ferrocyanide and dissolve it in 500 ml of deionized water. Stir for 2 hours under nitrogen protection. This is referred to as solution A.

[0035] Step 2: Weigh 0.21 mol of ferrous sulfate, 0.07 mol of manganese sulfate, 0.005 mol of nickel sulfate, 0.015 mol of zinc sulfate, 0.01 mol of citric acid and 0.3 mol of sodium citrate and dissolve them in 500 ml of deionized water, and stir for 1 hour under nitrogen protection, which is recorded as solution B;

[0036] Step 3: Weigh 0.7 mol sodium citrate, 0.03 mol citric acid and 2% vinyltrimethoxysilane and dissolve them in 300 ml deionized water. Stir for half an hour under nitrogen protection, and record it as solution C.

[0037] Step 4: Add liquid A and liquid B to solution C simultaneously through a peristaltic pump, wherein the dripping rate of liquid A and liquid B is 10 ml / min, the mechanical stirring speed of solution C is 300 r / min, and the temperature of solution C is maintained at 25°C. After solution A and solution B are added, solution C is stirred for 12 hours under nitrogen protection;

[0038] Step 5: The reactant obtained in step 4 was centrifuged, washed with deionized water for 3 times, and then vacuum dried at 120° C. for 12 h to obtain a product, which was recorded as FMNZ-1;

[0039] Example 2

[0040] The difference from Example 1 is that 0.21 mol of ferrous sulfate, 0.07 mol of manganese sulfate, 0.005 mol of nickel sulfate and 0.015 mol of zinc sulfate in step 2 are replaced by 0.195 mol of ferrous sulfate, 0.065 mol of manganese sulfate, 0.01 mol of nickel sulfate and 0.03 mol of zinc sulfate, and the rest is the same as Example 1. The prepared product is recorded as FMNZ-2;

[0041] Example 3

[0042] The difference from Example 1 is that 0.21 mol of ferrous sulfate, 0.07 mol of manganese sulfate, 0.005 mol of nickel sulfate and 0.015 mol of zinc sulfate in step 2 are replaced by 0.18 mol of ferrous sulfate, 0.06 mol of manganese sulfate, 0.02 mol of nickel sulfate and 0.04 mol of zinc sulfate, and the rest is the same as Example 1. The prepared product is recorded as FMNZ-3;

[0043] Comparative Example 1:

[0044] The difference from Example 1 is that 0.21 mol of ferrous sulfate, 0.07 mol of manganese sulfate, 0.005 mol of nickel sulfate and 0.015 mol of zinc sulfate in step 2 are replaced by 0.3 mol of ferrous sulfate, and the rest are the same as Example 1. The prepared product is recorded as FM-1.

[0045] Comparative Example 2:

[0046] The difference from Example 1 is that citric acid is not added in step 2, and citric acid and vinyltrimethoxysilane are not added in step 3. The rest is the same as Example 1, and the prepared product is recorded as FMNZ-4.

[0047] Battery Assembly:

[0048] The iron-based multi-doped Prussian blue positive electrode material, conductive carbon and polyvinylidene fluoride binder prepared in Example 1-3 and Comparative Example 1-2 were mixed into a slurry, coated on an aluminum foil, and vacuum dried in a vacuum oven at 120°C for 16 hours to obtain a positive electrode sheet. A button cell was assembled with a metal sodium sheet as the negative electrode, Grade GF / A glass fiber as the separator, and 1 mol / LNaPF6 / PC+EMC (PC:EMC=1:1) containing 5 wt% of the additive FEC as the electrolyte for constant current charge and discharge tests, with a test voltage range of 2 to 3.8V.

[0049] Test method:

[0050] Table 1: All battery assemblies were completed in a glove box (O2 wt% ≤ 0.01, H2O wt% ≤ 0.01). The constant current charge and discharge test and long cycle test voltage windows of CR2032 button batteries were both 2-3.8V. The initial rate was 0.1C, and it became 1C after one charge and discharge cycle. The test results are shown in the table below.

[0051]

[0052] Table 2: ICP of the vacuum dried material was measured. The test results are shown in the following table

[0053] <![CDATA[Ni 2+ (ppm)]]> <![CDATA[Zn 2+ (ppm)]]> Example 1 731.95 3918.44 Example 2 1370.44 8102.81 Example 3 2002.6 13660.93

[0054] in conclusion:

[0055] like Figure 1 As shown, the Prussian blue positive electrode material prepared in Example 2 has a cubic shape, and the particle size is uniform, with a particle size of about 1 to 2 μm. Figure 2 As shown, the Prussian blue materials synthesized in each embodiment are all in a monoclinic phase, wherein the crystal is stretched due to the internal stress of the crystal, and the corresponding peak shape of the (400) crystal plane changes. Figure 3 As shown, increasing the doping amount of nickel and zinc increases the crystallinity of the characteristic peak of the monoclinic phase (400) crystal plane, among which Example 2 has the highest crystallinity. Figure 4 As shown, the initial specific capacity of the Prussian blue cathode material prepared in Example 2 at a rate of 0.1C is 156.33 mAh / g. Figure 5As shown, compared with Comparative Example 1, as the amount of nickel-zinc doping increases, the long cycle performance of the three embodiments is improved successively, and the cycle performance is significantly better than that of Comparative Example 1. Figure 6 As shown, the capacity retention rate of the Prussian blue positive electrode material prepared in Example 1 and Comparative Example 2 after 400 cycles is basically close, and no obvious attenuation occurs. As shown in Table 1, as the nickel and zinc doping amounts increase, the particle size decreases accordingly. In Example 3, the total inert ion doping amount is close to 20%, and the initial specific capacity is about 150 mAh / g. Compared with Comparative Example 2, the specific capacity of Example 1 is significantly improved.

[0056] In summary, when the total amount of nickel and zinc doping is adjusted to about 13%, a balance between specific capacity and cycle performance can be achieved, that is, a high specific capacity is maintained while having a certain long cycle life. This shows that the high-crystallinity Prussian blue analogue obtained by the invention has low defects and a stable crystal structure, which helps to reduce the structural collapse and performance degradation during the battery cycle. Due to the action of the auxiliary agent and the silane coupling agent, the surface of Prussian blue is combined with the carboxylic acid ligand, so the specific capacity is further improved.

[0057] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a high-capacity and long-life iron-based multinary doped Prussian blue positive electrode material, It is characterized in that The following steps are involved: Step 1, dissolving sodium ferrocyanide in deionized water to obtain solution A; Dissolving a transition metal salt, a complexing agent and an auxiliary agent in deionized water to obtain a solution B, wherein the transition metal salt comprises one or a combination of two of a ferric salt and a ferrous salt, one or a combination of one or more of a nickel salt, a copper salt and a zinc salt, and a manganese salt; Adding an additive and a silane coupling agent to deionized water and mixing well to obtain a solution C, wherein the additives in both the solution B and the solution C contain a carboxylic acid group; Step 2: Add solution A and solution B to solution C simultaneously and stir to perform a co-precipitation reaction, centrifuge, wash, and vacuum dry to obtain a long-life iron-based multinary doped Prussian blue positive electrode material; The above steps are all carried out under the protection of inert gas.

2. The preparation method according to claim 1, Features: The concentration of sodium ferrocyanide in solution A is 0.1~0.4mol / L.

3. The preparation method according to claim 1, Features: In solution B, the iron salt, ferrous salt, nickel salt, copper salt and zinc salt are independently selected from any one or more combinations of chloride, sulfate, nitrate and acetate.

4. The preparation method according to claim 1, Features: The ratio of the total molar amount of the transition metal salt to the molar amount of sodium ferrocyanide is 0.5-2.

5. The preparation method according to claim 1, Features: In solution B, the total molar amount of ferric salt and ferrous salt is 50% to 90% of the total molar amount of transition metal salt, the molar amount of manganese salt is 5% to 40% of the total molar amount of transition metal salt, the molar amount of nickel salt is 0 to 20% of the total molar amount of transition metal salt, the molar amount of copper salt is 0 to 20% of the total molar amount of transition metal salt, and the molar amount of zinc salt is 0 to 20% of the total molar amount of transition metal salt; the molar ratio of the complexing agent to the transition metal cation in the transition metal salt is 1 to 3:1, and the molar ratio of the auxiliary agent to the complexing agent is 1:5 to 30.

6. The preparation method according to claim 1, Features: Solution C also includes a complexing agent.

7. The preparation method according to claim 1 or 6, Features: The complexing agent includes one or a combination of sodium citrate, sodium EDTA, and sodium pyrophosphate; the auxiliary agent includes one or a combination of citric acid, tartaric acid, and malic acid; and the silane coupling agent includes one or a combination of vinyl silane coupling agent, amino silane coupling agent, methacryloxy silane coupling agent, epoxy silane coupling agent, and mercapto silane coupling agent.

8. The preparation method according to claim 1, Features: In step 2, the dropwise addition rate of solution A and solution B is 1-20 ml / min, the reaction is carried out under mechanical stirring at 300-900 r / min, the reaction temperature is 25° C.-50° C., and the reaction time is 12-24 h.

9. The preparation method according to claim 1, Features: In step 2, the vacuum drying temperature is 100~170℃, drying time is 12h~48h.

10. The preparation method according to claim 6, Features: The mass fraction of the silane coupling agent in the solution C is 1% to 20%, the molar ratio of the complexing agent to the transition metal cation in the transition metal salt is 1 to 6:1, and the molar ratio of the auxiliary agent to the complexing agent is 1:5 to 30.