Method for recovering and preparing industrial lithium carbonate from battery material raffinate
By using rare earth-based fluorine dehydrator and deep purification process in lithium battery raffinate, combined with lithium precipitation and lithium phosphate precipitation steps, the problems of low lithium carbonate recovery and high impurities in the prior art are solved, and high purity is achieved , high recovery rate of industrial grade 0 lithium carbonate preparation reduces production costs and environmental impact.
Patent Information
- Application Number
- CN202411099979.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art cannot effectively recover and prepare lithium carbonate that meets the industrial grade 0 standard, and there are high cost and high impurity problems, especially when the lithium content and fluorine content in lithium battery raffinate are low.
The defluorination treatment is carried out by rare earth-based fluorine dehydrant, combined with deep purification and multiple filtration separation, through the lithium precipitation steps of lithium precipitation and lithium phosphate, combined with agitation and drying process, the purity and recovery rate of lithium carbonate are improved, meeting the industrial grade 0 standards.
It significantly improves the recovery rate of lithium metal and the purity of lithium carbonate, reduces the fluorine content and impurity content, meets the industrial grade 0 standards, and reduces production costs and environmental impacts.
Smart Images

Figure CN118993113A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of waste battery recycling and reprocessing, and more specifically to a method for recovering and preparing industrial lithium carbonate from battery material raffinate. Background Art
[0002] The development of new energy batteries has solved a large degree of energy demand for mankind. At present, the new energy batteries produced on a large scale in the market are mainly lead-acid batteries, nickel-metal hydride batteries, lithium batteries and sodium batteries. Lithium-ion batteries have become the battery with the highest market share in the new energy battery market due to their advantages such as high energy density, long cycle life, low environmental pollution and recyclability, and have good development prospects in the future.
[0003] Elements such as cobalt, nickel, manganese, lithium, iron and phosphorus in lithium batteries can be recycled and used as battery raw materials; at present, as the second-generation batteries are about to retire, the development momentum of lithium battery recycling is good. Traditional lithium battery recycling methods are generally divided into pyrometallurgical recycling and wet recycling. Pyrometallurgical recycling has great environmental pollution and low recovery rate; wet recycling has the advantages of low environmental pollution, simple process and high product quality, so wet recycling has become more and more the mainstream battery recycling method. Wet recycling is a relatively mature process for recovering metal elements such as cobalt, nickel or manganese by leaching and extraction. Due to the chemical properties of lithium, the cost of recovery through extraction is high and the process is difficult. However, based on the property that lithium and carbonate can produce precipitation, lithium metal can be recovered. However, the lithium content in the extract raffinate is generally low (1-5g / L), the direct precipitation cost is high and the yield is low. After increasing the lithium concentration by evaporation to precipitate the salt in the extract raffinate, a saturated solution with a high lithium concentration is used for reprecipitation. This is a preferred lithium recovery method.
[0004] According to the relevant provisions of the national standard "Lithium Carbonate" (GB / T11075-2013), industrial-grade lithium carbonate can be divided into three grades: Industrial lithium carbonate grade 0 (Li 2 CO 3 -0):Li 2 CO 3 Content ≥99.2%; Industrial lithium carbonate grade 1 (Li 2 CO 3 -1):Li 2 CO 3 Content ≥99.0%; Industrial lithium carbonate grade 2 (Li 2 CO 3 -2):Li 2 CO 3 Content ≥98.5%.
[0005] However, the impurities in the currently recycled industrial-grade lithium carbonate products are too high and cannot meet the standards of industrial grade 0 lithium carbonate.
[0006] For example, the Chinese patent with patent number CN2021108142462 announced on November 2, 2021, discloses a method for recovering and preparing crude lithium carbonate from battery material raffinate; the patent uses a zirconium-based defluorinating agent for defluorination, the control process is cumbersome, occupies a large production site, and has high initial investment. The patent does not involve oil removal, deep purification, stirring and washing processes, and the output product has a high impurity content and cannot meet the industrial grade 0 lithium carbonate standard.
[0007] Therefore, it is necessary to provide a method for recovering and preparing industrial grade 0 lithium carbonate from battery material raffinate, which has low preparation cost, and the recovered and prepared lithium carbonate has low fluorine content, high recovery rate and high purity. Summary of the invention
[0008] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for recovering and preparing industrial lithium carbonate from battery material raffinate. The lithium carbonate obtained by this method has a main content of more than 99.25%, which not only meets the quality standard of industrial lithium carbonate grade 0, but also significantly improves the recovery efficiency of lithium metal and promotes the recycling of resources; and the method adopts a rare earth-based defluorinating agent, which effectively reduces the fluorine content in the lithium carbonate to below 0.01%, thereby further improving the purity of the product.
[0009] To solve the above problems, the present invention adopts the following technical solutions.
[0010] A method for recovering and preparing industrial lithium carbonate from battery material raffinate, comprising the steps of: S1: removing oil and phosphorus from the battery material raffinate, and then adding a rare earth-based defluorinating agent to remove fluorine to obtain a defluorinated liquid; S2: adding alkaline liquid auxiliary material to the defluorinated liquid in step S1 to remove heavy metals, filtering and separating to obtain precipitated heavy metal liquid and precipitated heavy metal slag, adjusting the pH of the precipitated metal liquid to neutral, performing falling film evaporation and MVR forced circulation evaporation, and then performing thickening and centrifugation operations to obtain sodium sulfate product and evaporation mother liquor, and performing thickening operations on the evaporation mother liquor to obtain evaporation mother liquor underflow and evaporation mother liquor supernatant; S3: deep purification of the supernatant of the evaporated mother liquor, multiple filtration separation, and adding liquid carbonate to the filtrate to obtain primary lithium carbonate and lithium precipitation mother liquor through lithium precipitation; S4: After adding sulfuric acid to the lithium precipitation mother liquor to remove carbonate, adding alkali to adjust the pH to neutral; then subjecting it to MVR forced circulation evaporation to obtain sodium sulfate and secondary evaporation mother liquor; adding liquid carbonate to the secondary evaporation mother liquor to perform secondary lithium precipitation to obtain secondary lithium precipitation lithium carbonate product and secondary lithium precipitation mother liquor; adding phosphate to the secondary lithium precipitation mother liquor to perform phosphate lithium precipitation, filtering to obtain lithium phosphate and phosphate lithium precipitation mother liquor, and removing impurities from the phosphate lithium precipitation mother liquor wastewater before discharge; S5: The primary lithium carbonate is stirred, washed, centrifuged and dried to obtain industrial-grade lithium carbonate.
[0011] Furthermore, in the battery material raffinate, the lithium content is 1-6 g / L, the sodium content is 40-80 g / L, the oil content is 20-100 mg / L, the fluorine content is 30-100 mg / L, the phosphorus content is 10-50 mg / L, and the chlorine content is 0.5-3 g / L.
[0012] Furthermore, the degreasing agent added in the degreasing operation is activated carbon that has been slurried, and the mass ratio of the added activated carbon to the battery material raffinate is 3%-8%.
[0013] Furthermore, the bottom water of the activated carbon slurry is the ternary battery material raffinate raw material, the activated carbon is wood powder activated carbon, the reaction process is at room temperature, and the reaction time is 0.5-2h.
[0014] Furthermore, the dephosphorization agent added in the dephosphorization operation refers to a liquid dephosphorization agent with a mass concentration of 10%-20%, the mass ratio of the dephosphorization agent added to the battery material raffinate is 3%-8%, the temperature of the dephosphorization reaction is room temperature, the pH is 3-6, and the reaction time is 0.5-2h; the dephosphorization agent is specifically one or a mixture of ferrous sulfate, polyferric sulfate or aluminum sulfate.
[0015] Furthermore, the mass ratio of the rare earth-based defluorinating agent added to the battery material raffinate is 3%-8%, the reaction temperature is room temperature, the reaction pH is 3-7, and the reaction time is 0.5-2h.
[0016] Furthermore, the rare earth content of the rare earth-based defluorinating agent is 30%-40%; the rare earth element is mainly one or a mixture of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium or dysprosium.
[0017] Furthermore, the alkaline liquid auxiliary material is one or a mixture of sodium carbonate, calcium carbonate or sodium hydroxide, the reaction temperature of the heavy metal is room temperature, the reaction pH is 8-14, and the reaction time is 0.5-3h.
[0018] Furthermore, the liquid carbonate is one or a mixture of sodium carbonate, calcium carbonate, magnesium carbonate or potassium carbonate; the purification temperature is 60-100°C, the purification pH is 9-14, the purification time is 1-4h, and the excess coefficient of liquid carbonate addition is 1.0~2.0.
[0019] Furthermore, the phosphate is one or a mixture of sodium phosphate, aluminum phosphate or ammonium phosphate; the temperature of lithium phosphate precipitation is 60-100°C, the pH is 8-14, the time of lithium phosphate precipitation is 1-3h, and the excess coefficient of phosphate addition is 1.0~2.0.
[0020] The above technical solution is specifically as follows: A method for recovering and preparing industrial lithium carbonate from battery material raffinate, comprising the steps of: (1) Oil removal: Add wood activated carbon to the battery material raffinate to obtain an oil-removed liquid with an oil content of less than 5 mg / L. The obtained oil-removed residue is sold; (2) Phosphorus removal: Add a liquid dephosphorizing agent to the deoiled liquid to obtain a dephosphorized liquid with a phosphorus content of less than 10 mg / L. The resulting slag is discarded after treatment; (3) Fluorine removal: adding a defluorinating agent to the dephosphorized liquid to obtain a defluorinated liquid with a fluorine content of less than 1 mg / L, and the resulting slag is discarded after treatment; (4) Heavy metals: add alkaline liquid auxiliary materials to the defluorinated liquid to remove heavy metals. After the heavy metals are precipitated, they are separated by filter press to obtain heavy metal liquid and heavy metal slag, and the heavy metal slag is recovered; (5) Acid and alkali adjustment: Add acid and alkali to the heavy metal solution to adjust the pH of the solution to neutral; (6) Evaporation and concentration: The solution after acid and alkali adjustment is evaporated by falling film evaporation and MVR forced circulation until the mother liquor concentration reaches the expected concentration, and then thickening and centrifugation operations are performed to obtain sodium sulfate product and evaporation mother liquor. The evaporation mother liquor is subjected to a thickening operation to obtain an evaporation mother liquor underflow and an evaporation mother liquor supernatant. The evaporation mother liquor underflow is returned to the thickening section; (7) Deep purification: A small amount of carbonate and liquid alkali is added to the supernatant of the evaporation mother liquor for deep purification, followed by multiple filtration separations through a filter press and a precision filter, and the filter residue is used to recover heavy metals; (8) lithium precipitation: adding the filtrate obtained in step (7) into a liquid carbonate solution to produce a primary lithium carbonate product and a lithium precipitation mother liquor through a high temperature precipitation reaction; (9) Evaporation of lithium precipitation mother liquor: adding sulfuric acid to the lithium precipitation mother liquor obtained in step (8) to remove carbonate, then adding alkali to adjust the pH to neutral, and subjecting the mixture to MVR forced circulation evaporation to produce sodium sulfate and secondary evaporation mother liquor; (10) Secondary lithium precipitation: adding liquid carbonate to the secondary evaporation mother liquor, and producing secondary lithium carbonate and secondary lithium precipitation mother liquor after high temperature precipitation reaction; (11) Treatment of secondary lithium precipitation mother liquor: adding phosphate to the secondary lithium precipitation mother liquor produced in step (10) for deep lithium precipitation, performing solid-liquid separation after deep lithium precipitation to obtain phosphate lithium precipitation mother liquor and lithium phosphate, wherein the lithium phosphate is sold as a by-product, and the phosphate lithium precipitation mother liquor is discharged after wastewater impurity removal treatment; (12) lithium carbonate washing: washing the primary lithium carbonate obtained in step (8) and the secondary lithium carbonate prepared in step (10) twice in countercurrent and then centrifuging for solid-liquid separation to obtain primary lithium carbonate wet material and secondary lithium carbonate wet material; (13) Drying and packaging of lithium carbonate: The primary lithium carbonate wet material and the secondary lithium carbonate wet material obtained in step (12) are dried in a dryer respectively, and then mixed and packaged to obtain an industrial-grade lithium carbonate product.
[0021] Furthermore, in the battery material raffinate, the lithium content is 1-6 g / L, the sodium content is 40-80 g / L, the oil content is 20-100 mg / L, the fluorine content is 30-100 mg / L, the phosphorus content is 10-50 mg / L, and the chlorine content is 0.5-3 g / L.
[0022] Furthermore, in step (1), the wood activated carbon is wood powdered activated carbon, and the mass ratio of the added wood activated carbon to the battery material raffinate is 3%-8%, and the activated carbon residue after oil removal is sold for recycling.
[0023] Furthermore, in step (1), the activated carbon is used after slurry preparation, the slurry bottom water is the raw material of the ternary battery material raffinate, the reaction temperature of the oil removal operation is room temperature, and the reaction time is 0.5-2h.
[0024] Furthermore, in step (2), the dephosphorizing agent is one or a mixture of ferrous sulfate, polyferric sulfate or aluminum sulfate; the dephosphorizing agent is a liquid dephosphorizing agent with a mass concentration of 10%-20%, a mass ratio of the dephosphorizing agent added to the battery material raffinate of 3%-8%, a reaction temperature of room temperature, a reaction pH of 3-6, and a reaction time of 0.5-2h.
[0025] Furthermore, in step (3), the defluorination agent is a rare earth-based defluorination agent, the rare earth content is 30%-40%, and the rare earth metal is mainly one or a mixture of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium or dysprosium.
[0026] Furthermore, the mass ratio of the rare earth-based defluorinating agent added to the battery material raffinate is 3%-8%, the reaction temperature of the defluorinating operation is room temperature, the reaction pH is 3-7, and the reaction time is 0.5-2h.
[0027] Furthermore, in step (4), the alkaline liquid auxiliary material used for the heavy metal is one or a mixture of sodium carbonate, calcium carbonate or sodium hydroxide, the reaction temperature for the heavy metal operation is room temperature, the reaction pH is 8-14, and the reaction time is 0.5-3h.
[0028] Furthermore, in step (5), the acid used for acid adjustment is concentrated sulfuric acid with a mass concentration of 90%-98%, the alkali used for alkali adjustment is liquid sodium hydroxide with a mass concentration of 20%-32%, the reaction is a continuous reaction, and the material residence time is 1-3h.
[0029] Furthermore, in step (6), the evaporation operation is to first adopt falling film circulation evaporation and then adopt MVR forced circulation evaporation; when the lithium concentration of the mother liquor is 10-20 g / L, the evaporated mother liquor is passed through a thickener, a centrifuge and a thickener for solid enrichment and solid-liquid separation operations, and the solid content in the final evaporated mother liquor is less than 0.5%.
[0030] Furthermore, in step (7), the carbonate used for deep purification is one or a mixture of sodium carbonate, calcium carbonate, magnesium carbonate or potassium carbonate, the purification temperature of the deep purification operation is 60-100°C, the purification pH is 9-14, and the purification time is 1-4h.
[0031] Furthermore, in step (8), the liquid carbonate is one or a mixture of sodium carbonate, ammonium carbonate or potassium carbonate, the lithium precipitation temperature of the lithium precipitation operation is 70-100°C, the lithium precipitation time is 0.5-2h, the addition of carbonate is carried out by reverse addition method, and the excess coefficient of carbonate addition is 1.0-2.0.
[0032] Furthermore, in step (11), the phosphate is one or a mixture of sodium phosphate, aluminum phosphate or ammonium phosphate, the deep lithium precipitation temperature is 60-100°C, the pH is 8-14, the deep lithium precipitation time is 1-3h, and the excess coefficient of phosphate addition is 1.0-2.0.
[0033] Furthermore, in step (11), the lithium content in the phosphate lithium precipitation mother liquor is ≤0.2 g / L.
[0034] Furthermore, in step (12), the lithium carbonate stirring and washing liquid-solid ratio is 3-6:1, the stirring and washing temperature is 60-100° C., and the stirring and washing time is 20-80 min.
[0035] Furthermore, in step (13), the lithium carbonate is dried using a disc dryer, and the dryer uses a steam coil heating method to achieve heat exchange and evaporate and remove moisture from the product. The drying environment temperature is 100-150° C. and the drying time is 1-4 hours.
[0036] Compared with the prior art, the advantages of the present invention are: 1. The method for recovering and preparing industrial lithium carbonate from battery material raffinate provided by the present invention can significantly improve the recovery rate of lithium metal and promote the recycling of resources; and the main content of lithium carbonate obtained by this method can reach more than 99.25%; at the same time, through deep purification and stirring and washing, the calcium content of the prepared lithium carbonate product is less than 0.025%, the sulfate content is less than 0.2%, the fluorine content is less than 0.01%, and the moisture content is less than 0.2%, thereby improving the purity of the lithium carbonate product, so that all its indicators meet the product standards of industrial grade 0 lithium carbonate.
[0037] 2. The present invention uses a rare earth-based defluorinating agent in the recovery of lithium metal from battery materials; the use of the rare earth-based defluorinating agent makes the fluorine content of the lithium carbonate product prepared by the present invention lower than 0.01%, which significantly improves the purity of the lithium carbonate.
[0038] 3. The process adopted by the present invention has the advantages of short process, low initial investment, low production cost, high lithium recovery rate and high product quality.
[0039] Fourth, the present invention adopts falling film circulation evaporation and forced circulation evaporation process to increase the concentration of lithium ions in the solution after acid and alkali adjustment, and reduces the salt content in the evaporation mother liquor to less than 0.5% through thickening, centrifugation, concentration and other operations, thereby reducing the interference of impurities on subsequent treatment processes and improving the purity of the product.
[0040] 5. In the present invention, the lithium precipitation mother liquor is separated again after acid-base adjustment and re-evaporation to obtain sodium sulphate and lithium carbonate products, which reduces the open circuit volume of the lithium precipitation mother liquor by 70%, significantly reduces the discharge volume of the lithium precipitation mother liquor, reduces the waste treatment cost and environmental impact; and this operation increases the lithium recovery rate by 0.5%, reducing the waste of resources.
[0041] 6. In the present invention, industrial lithium carbonate undergoes two countercurrent washings, the washing water is evaporation condensation water, the washing mother liquor is used for auxiliary material configuration, and no other water is introduced during the washing process, thereby realizing the recycling of resources, reducing the demand for new water in the preparation process, and avoiding the introduction of new impurities, thereby ensuring the quality of the product. Moreover, after washing, the sulfate content in the lithium carbonate is less than 0.2%, and the sodium content is less than 0.08%, which significantly improves the purity of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 The present invention is a process flow chart for recovering and preparing industrial lithium carbonate from battery material raffinate. DETAILED DESCRIPTION
[0043] Example 1
[0044] Under normal temperature and pressure conditions, add 3‰ of slurry-prepared activated carbon to the battery material raffinate, react for 0.6h, filter press to obtain deoiled liquid and filter press residue. The filter press residue is sold outside; the deoiled liquid is pumped into the dephosphorization tank, and a dephosphorization agent with a mass concentration of 15% is added according to the ratio of dephosphorization agent to deoiled liquid of 4‰, and the dephosphorization pH is adjusted to 4.5. After 0.5h of reaction, filter press to obtain dephosphorization slag and dephosphorization liquid. The dephosphorization liquid is pumped into the defluorination tank, and after adding alkali to adjust the pH to 5.0, a defluorination agent is added according to the mass ratio of solution to defluorination agent of 3.5‰ for defluorination. After 0.6h of reaction, filter press to obtain defluorination slag and defluorination liquid. The defluorination liquid is pumped into the heavy metal tank, and an alkaline liquid is added to adjust the pH to 12.0. After 1h of reaction, filter press to obtain heavy metal slag and heavy metal liquid. The heavy metal slag obtained by sedimentation is used to recover heavy metals; concentrated sulfuric acid with a mass fraction of 98% and sodium hydroxide solution with a mass concentration of 32% are added to the heavy metal post-liquid for adjustment, and the acid adjustment and alkali adjustment time are controlled to be 1h respectively. After the pH is adjusted to 7.0, it is sent to the evaporation equipment for falling film evaporation and forced circulation evaporation. When the lithium concentration in the mother liquor of forced circulation evaporation reaches 12g / L, it is subjected to thickening operation and centrifugal operation to obtain the glauber powder product and the evaporation mother liquor. The mother liquor is thickened by the thickener to obtain the evaporation mother liquor underflow and the evaporation mother liquor supernatant. The evaporation mother liquor underflow returns to the thickening section, and after the evaporation mother liquor supernatant is pumped into the deep purification tank, sodium carbonate and liquid alkali are added to adjust the pH of the liquid in the deep purification tank to 12.0, and the purification tank temperature is adjusted to 95℃. After reacting for 2h, the purification slag and the purified post-liquid are obtained by pressure filtration. Purify the slag and recycle it; pump the purified liquid into the lithium precipitation tank, add a sodium carbonate solution with a mass concentration of 25% in advance according to the theoretical amount of 1.1 times, adjust the temperature to 90℃, react for 1h and filter press to obtain a wet lithium carbonate product and a mother liquor of lithium precipitation. After adding sulfuric acid to the mother liquor of lithium precipitation to remove carbonate, add alkali to adjust the pH of the solution to neutral, and then force circulation evaporation to produce glauber powder and a second evaporation mother liquor. Pass the second evaporation mother liquor into the lithium precipitation tank, and add sodium phosphate to the lithium precipitation tank for secondary lithium precipitation to obtain a wet lithium carbonate product and a mother liquor of lithium precipitation. Add trisodium phosphate to the mother liquor of lithium precipitation according to the theoretical amount of 1.1 times, adjust the reaction pH to 10.0, heat to 80℃, react for 2h and filter press to obtain a lithium phosphate product and a sodium phosphate lithium precipitation liquid. The lithium phosphate product is recovered, and the sodium phosphate lithium precipitation liquid is discharged after phosphorus removal and COD removal.
[0045] The lithium carbonate product was stirred and washed twice, with a liquid-solid ratio of 3:1, heated to 70°C, stirred and washed for 30 minutes, and centrifuged. After centrifugation, the lithium carbonate product was dried and packaged. The lithium recovery rate was 99.5%. ; It can be seen from Table 4, Table 5 and Table 6 that the primary lithium carbonate product meets the requirements of Level 0 of the national industrial grade lithium carbonate standard (GB / T11075-2013).
[0046] Example 2
[0047] Under normal temperature and pressure conditions, add 3.5‰ of slurry-prepared activated carbon to the battery material raffinate, react for 0.5h, filter press to obtain filter press residue and deoiled liquid. The filter press residue is sold outside; the deoiled liquid is pumped into the dephosphorization tank, and a dephosphorization agent with a mass concentration of 15% is added according to the ratio of dephosphorization agent to deoiled liquid of 3.5‰, and the dephosphorization pH is adjusted to 4.0. After 0.7h of reaction, filter press is performed to obtain dephosphorization slag and dephosphorization liquid. The dephosphorization liquid is pumped into the defluorination tank, and after adding alkali to adjust the pH to 4.5, a defluorination agent is added according to the mass ratio of solution to defluorination agent of 3.0‰ for defluorination. After 0.5h of reaction, filter press is performed to obtain defluorination slag and defluorination liquid. The defluorination liquid is pumped into the heavy metal tank, and an alkaline liquid is added to adjust the pH to 11.0. After 1.5h of reaction, filter press is performed to obtain heavy metal slag and heavy metal liquid. The heavy metal slag obtained by sedimentation is used to recover heavy metals. Concentrated sulfuric acid with a mass fraction of 98% and sodium hydroxide solution with a mass concentration of 32% are added to the heavy metal post-liquid for adjustment. The acid adjustment and alkali adjustment time are controlled to be 1.5h respectively. After the pH is adjusted to 7.0, it is sent to the evaporation equipment for falling film evaporation and forced circulation evaporation. When the lithium concentration in the mother liquor of forced circulation evaporation reaches 14g / L, it is subjected to thickening and centrifugal operation to obtain the glauber powder product and the evaporation mother liquor. The mother liquor is thickened by the thickener to obtain the evaporation mother liquor underflow and the evaporation mother liquor supernatant. The evaporation mother liquor underflow returns to the thickening section. After the evaporation mother liquor supernatant is pumped into the deep purification tank, sodium carbonate and liquid alkali are added to adjust the pH of the liquid in the deep purification tank to 13.0. At the same time, the purification tank temperature is adjusted to 90℃. After reacting for 1.5h, it is filtered to obtain the purified slag and the purified post-liquid. The purified slag is recovered; the purified liquid is pumped into a lithium precipitation tank, and a sodium carbonate solution with a mass concentration of 30% is added to the lithium precipitation tank in advance according to 1.2 times the theoretical amount, and the temperature is adjusted to 95°C. After reacting for 1.5 hours, filter pressure is obtained to obtain a primary lithium precipitation lithium carbonate wet product and a primary lithium precipitation mother liquor.
[0048] After adding sulfuric acid to the primary lithium precipitation mother liquor to remove carbonate ions, add alkali to adjust the pH to neutral, and then force circulation evaporation to produce alum and secondary evaporation mother liquor. The secondary evaporation mother liquor is passed into the lithium precipitation tank, and phosphate is added to the lithium precipitation tank for secondary lithium precipitation to obtain secondary lithium precipitation lithium carbonate wet product and secondary lithium precipitation mother liquor. Add trisodium phosphate to the secondary lithium precipitation mother liquor according to 1.2 times the theoretical amount, adjust the reaction pH to 11.5, the temperature to 90°C, react for 2.5 hours, and filter press to obtain lithium phosphate product and sodium phosphate lithium precipitation liquid. The lithium phosphate product is recovered, and the sodium phosphate lithium precipitation liquid is filtered and discharged after the COD is qualified.
[0049] The wet lithium carbonate product of the first precipitation is stirred and washed twice, with the stirring and washing liquid-solid ratio controlled at 4:1, the temperature at 65℃, and centrifuged after stirring and washing for 40 minutes. After centrifugation, the wet lithium carbonate product of the first precipitation is dried and packaged to produce industrial-grade lithium carbonate. The industrial-grade lithium carbonate meets the national industrial-grade lithium carbonate standard (GB / T11075-2013) level 0 requirements. The lithium recovery rate is 99.5%. ; It can be seen from Table 9, Table 10 and Table 6 that the primary lithium carbonate product meets the requirements of Level 0 of the national industrial grade lithium carbonate standard (GB / T11075-2013).
[0050] Comparative Example 1 Under normal temperature conditions, add 3% zirconium-based defluorinating agent to the battery material raffinate, start stirring, control the defluorination pH to 4.5, and filter the defluorination slurry after a reaction time of 0.5h. The defluorinating agent carrying fluorine is regenerated by 0.5mol / L sodium hydroxide solution to remove fluorine. The regenerated defluorinating agent is slurried by the battery material raffinate and returned to the defluorination section for recycling. Add a dephosphorizing agent solution with a mass concentration of 15% to the defluorinated liquid obtained by filter pressing separation, control the pH to 3.99, and remove phosphorus for 30min. The dephosphorizing slurry is separated by filter pressing, and the dephosphorizing liquid is collected. Add lithium precipitation mother liquor to the dephosphorizing liquid (the mass ratio of the dephosphorizing liquid to the lithium precipitation mother liquor is 3:1) to adjust the pH to 10.0 and the temperature to 60℃. After reacting for 60min, filter the heavy metal slurry to obtain nickel-containing heavy metal slag and heavy metal filter press liquid. The nickel-containing heavy metal slag is recovered by leaching.
[0051] Add 98% sulfuric acid to the heavy metal filter press liquid to adjust the pH to 4.0, then add 32% liquid alkali to adjust the pH to 7.0 to obtain the acid-base adjusted liquid, and evaporate the acid-base adjusted liquid through a two-effect circulation evaporator. The concentration ratio of the evaporation process is controlled to be 4 times to obtain the evaporation mother liquor. Add 30% sodium carbonate solution to the evaporation mother liquor according to 1.1 times the theoretical amount for lithium precipitation. The temperature of lithium precipitation is 80°C, the lithium precipitation time is 2h, and the evaporation mother liquor is added to the lithium precipitation container through multi-point scattering. The output lithium carbonate meets the national industrial grade lithium carbonate standard (GB / T11075-2013). The lithium recovery rate is 90%.
[0052] ; It can be seen from Table 14 and Table 6 that the industrial-grade lithium carbonate prepared in this embodiment is of the third-grade quality of industrial lithium carbonate.
[0053] It can be seen from Example 1, Example 2 and the comparative example that the quality of the lithium carbonate outputted by the present invention can reach the industrial grade 0 standard, while the lithium carbonate outputted by the comparative example only reaches the industrial grade 3 quality, and does not reach the industrial grade 0. Specifically embodied in that the main content of the product outputted by the present invention reaches more than 99.2%, the main content of the product outputted by the comparative example is less than 99%, the fluorine content of the lithium carbonate outputted by the present invention reaches less than 0.01%, and the comparative example is 0.015%, and the impurity content of sodium, sulfate, fluorine, etc. in the lithium carbonate outputted by the present invention is also much lower than the sodium, sulfate, and fluorine content in the lithium carbonate outputted by the comparative example. Moreover, the lithium recovery rate of lithium carbonate prepared by the present method can reach 99.5%, with high yield and low cost.
[0054] The above embodiments describe some details of the implementation of the present invention, but they should not be understood as limitations of the present invention. Those skilled in the art may change, modify, replace and modify the present invention within the scope of the present invention without departing from the principles and purpose of the present invention.
Claims
1. A method for recovering and preparing industrial lithium carbonate from battery material raffinate, characterized in that: Includes steps: S1: removing oil and phosphorus from the battery material raffinate, and then adding a rare earth-based defluorinating agent to remove fluorine to obtain a defluorinated liquid; S2: adding alkaline liquid auxiliary material to the defluorinated liquid in step S1 to remove heavy metals, filtering and separating to obtain heavy metal liquid and heavy metal slag, adjusting the pH of the liquid after precipitation of heavy metals to neutral, performing falling film evaporation and MVR forced circulation evaporation, and then performing thickening and centrifugation operations to obtain sodium sulfate product and evaporation mother liquor, and performing thickening operations on the evaporation mother liquor to obtain evaporation mother liquor underflow and evaporation mother liquor supernatant; S3: deep purification of the supernatant of the evaporated mother liquor, multiple filtration separation, and adding liquid carbonate to the filtrate to obtain primary lithium carbonate and lithium precipitation mother liquor through lithium precipitation; S4: After adding sulfuric acid to the lithium precipitation mother liquor to remove carbonate, adding alkali to adjust the pH to neutral; Subsequently, MVR forced circulation evaporation is performed to obtain sodium sulfate and secondary evaporation mother liquor; liquid carbonate is added to the secondary evaporation mother liquor to perform secondary lithium precipitation to obtain secondary lithium precipitation lithium carbonate product and secondary lithium precipitation mother liquor; phosphate is added to the secondary lithium precipitation mother liquor to perform phosphate lithium precipitation, and then lithium phosphate and phosphate lithium precipitation mother liquor are obtained by filtering, and the phosphate lithium precipitation mother liquor wastewater is treated to remove impurities and then discharged; S5: The primary lithium carbonate is stirred, washed, centrifuged and dried to obtain industrial-grade lithium carbonate.
2. A method for recovering industrial lithium carbonate from battery material raffinate according to claim 1, characterized in that: The battery material raffinate has a lithium content of 1-6 g / L, a sodium content of 40-80 g / L, an oil content of 20-100 mg / L, a fluorine content of 30-100 mg / L, a phosphorus content of 10-50 mg / L, and a chlorine content of 0.5-3 g / L.
3. A method for recovering industrial lithium carbonate from battery material raffinate according to claim 1, characterized in that: The degreasing agent added in the degreasing operation is activated carbon prepared by slurry preparation, and the mass ratio of the added activated carbon to the battery material raffinate is 3%-8%.
4. The method for recovering industrial lithium carbonate from battery material raffinate according to claim 1, characterized in that: The bottom water of the activated carbon slurry is the ternary battery material raffinate raw material, the activated carbon is wood powder activated carbon, the reaction process is at room temperature, and the reaction time is 0.5-2h.
5. The method for recovering industrial lithium carbonate from battery material raffinate according to claim 1, characterized in that: The dephosphorization agent added in the dephosphorization operation refers to a liquid dephosphorization agent with a mass concentration of 10%-20%, the mass ratio of the dephosphorization agent added to the battery material raffinate is 3%-8%, the temperature of the dephosphorization reaction is room temperature, the pH is 3-6, and the reaction time is 0.5-2h; the dephosphorization agent is specifically one or a mixture of ferrous sulfate, polyferric sulfate or aluminum sulfate.
6. The method for recovering industrial lithium carbonate from battery material raffinate according to claim 1, characterized in that: The mass ratio of the rare earth-based defluorinating agent added to the battery material raffinate is 3%-8%, the reaction temperature is room temperature, the reaction pH is 3-7, and the reaction time is 0.5-2h.
7. A method for recovering industrial lithium carbonate from battery material raffinate according to claim 6, characterized in that: The rare earth content of the rare earth-based defluorinating agent is 30%-40%; the rare earth element is mainly one or a mixture of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium or dysprosium.
8. The method for recovering industrial lithium carbonate from battery material raffinate according to claim 1, characterized in that: The alkaline liquid auxiliary material is one or a mixture of sodium carbonate, calcium carbonate or sodium hydroxide, the reaction temperature of the heavy metal is room temperature, the reaction pH is 8-14, and the reaction time is 0.5-3h.
9. The method for recovering industrial lithium carbonate from battery material raffinate according to claim 1, characterized in that: The liquid carbonate is one or a mixture of sodium carbonate, calcium carbonate, magnesium carbonate or potassium carbonate; the purification temperature is 60-100° C., the purification pH is 9-14, the purification time is 1-4 hours, and the excess coefficient of the liquid carbonate is 1.0-2.
0.
10. The method for recovering industrial lithium carbonate from battery material raffinate according to claim 1, characterized in that: The phosphate is one or a mixture of sodium phosphate, aluminum phosphate or ammonium phosphate; the temperature of lithium phosphate precipitation is 60-100°C, the pH is 8-14, the time of lithium phosphate precipitation is 1-3h, and the excess coefficient of phosphate addition is 1.0-2.0.