Method for removing sulfate radicals from battery-grade lithium carbonate and application of method

By removing the sulfate from lithium carbonate fine grinding and washing, the problem of high sulfate content in battery-grade lithium carbonate is solved, effectively reducing the sulfate content and improving product quality are achieved, and it is suitable for industrial production.

CN118993115APending Publication Date: 2024-11-22TIANQI LITHIUM SHEHONG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411187261.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the traditional lithium carbonate production process, the sulfate content in battery-grade lithium carbonate products is difficult to reduce, and often exceeds national standards, resulting in unqualified product quality.

Method used

The sulfate is removed by coarsely removing impurities from lithium carbonate and then grinding until the particle size D50 is 4 μm-7 μm, and stirring and washing and centrifuging, and drying after solid-liquid separation to remove sulfate and reduce its content.

Benefits of technology

Effectively reduce the sulfate content in battery-grade lithium carbonate, improve product quality, and is suitable for industrial production applications. The sulfate content is reduced from exceeding the standard of 800ppm to meeting the standard requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993115A_ABST
    Figure CN118993115A_ABST
Patent Text Reader

Abstract

The invention provides a method for removing sulfate radicals from battery-grade lithium carbonate and application of the method, and relates to the technical field of battery-grade lithium carbonate, and the method comprises the following steps: roughly removing sulfate radical impurities from lithium carbonate, then grinding the lithium carbonate until the particle size D50 is 4-7 microns to obtain a fine ground material, washing the fine ground material, and carrying out solid-liquid separation to obtain the battery-grade lithium carbonate. The technical problem that the content of sulfate radicals in the battery-grade lithium carbonate is difficult to effectively reduce in the prior art is solved, the technical effects of efficiently reducing the content of the sulfate radicals and remarkably improving the quality of the battery-grade lithium carbonate are achieved, and meanwhile the method has the advantages of being simple in process and easy to operate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of battery-grade lithium carbonate, and in particular to a method for removing sulfate from battery-grade lithium carbonate and application thereof. Background Art

[0002] In the traditional lithium carbonate production process, the sulfate content of the battery-grade lithium carbonate product obtained after two stirring and washing processes is often kept at a high level, resulting in the sulfate content failing to meet the standard and exceeding the national standard of 800ppm. Therefore, how to effectively reduce the sulfate content in battery-grade lithium carbonate products is a technical problem that needs to be solved urgently in the industry.

[0003] How to effectively improve the impact of sulfate peritectic caused by the lithium precipitation process through simple process adjustments, thereby improving the quality of battery-grade lithium carbonate products, is of great practical significance to enterprises.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One of the purposes of the present invention is to provide a method for removing sulfate from battery-grade lithium carbonate, which has a simple process and is easy to operate, and can effectively reduce the sulfate content in battery-grade lithium carbonate.

[0006] The second purpose of the present invention is to provide an application of a method for removing sulfate from battery-grade lithium carbonate, which is beneficial to improving the quality of battery-grade lithium carbonate products.

[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0008] In a first aspect, a method for removing sulfate from battery-grade lithium carbonate comprises the following steps:

[0009] The lithium carbonate is roughly ground to a particle size D50 of 4 μm-7 μm after sulfate impurities are removed to obtain a finely ground material, and the finely ground material is washed and solid-liquid separated to obtain the battery-grade lithium carbonate.

[0010] Furthermore, the lithium carbonate includes lithium carbonate generated by lithium precipitation.

[0011] Furthermore, the lithium carbonate is obtained by a lithium precipitation reaction between sodium carbonate and lithium sulfate.

[0012] Furthermore, the washing method includes stirring washing with water.

[0013] Furthermore, the solid content of the finely ground material during washing is ≤70%.

[0014] Furthermore, the stirring speed of the washing is 100r / min-120r / min, and the stirring time of the washing is 10min-20min;

[0015] Preferably, the reaction temperature of the washing is ≥95°C.

[0016] Furthermore, the solid-liquid separation method includes separation by centrifugation.

[0017] Furthermore, the centrifugal rotation speed is 1250r / min-1470r / min.

[0018] Furthermore, after the solid-liquid separation, the method further includes a step of drying the washed material.

[0019] A second aspect is an application of any of the methods described above in the production of lithium carbonate.

[0020] Compared with the prior art, the present invention has at least the following beneficial effects:

[0021] The method for removing sulfate from battery-grade lithium carbonate provided by the present invention comprises the following steps: after the sulfate impurities are roughly removed from the lithium carbonate, the lithium carbonate is ground to a particle size D50 of 4 μm-7 μm, so that the coated sulfate can be fully released, and after washing, the sulfate content is greatly reduced; the method of the present invention is not only simple in process and easy to operate, but also can efficiently reduce the sulfate content in the battery-grade lithium carbonate, effectively improve the quality of the lithium carbonate product, and is suitable for industrial production and application.

[0022] The application of the method for removing sulfate from battery-grade lithium carbonate provided by the present invention is beneficial to improving the quality of battery-grade lithium carbonate products. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 A schematic diagram of the production process of battery-grade lithium carbonate provided in one embodiment of the present invention. DETAILED DESCRIPTION

[0025] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] According to a first aspect of the present invention, there is provided a method for removing sulfate from battery-grade lithium carbonate, comprising the following steps:

[0027] The lithium carbonate is roughly ground to a particle size D50 of 4 μm-7 μm after sulfate impurities are removed to obtain a finely ground material, which is then washed and solid-liquid separated to obtain battery-grade lithium carbonate.

[0028] The lithium carbonate after rough impurity removal is finely ground to a particle size D50 of 4μm-7μm, and then washed, which can effectively remove sulfate and greatly reduce the sulfate content, and can reduce the sulfate content exceeding the standard (standard 800ppm) to within the qualified line.

[0029] Typical but non-limiting particle sizes D50 of finely ground lithium carbonate are, for example, 4 μm, 5 μm, 6 μm, and 7 μm. A suitable particle size D50 can ensure that the coated sulfate is fully released, thereby ensuring sufficient washing to remove the sulfate. If the particle size D50 is too small, the material will escape during centrifugal water removal, resulting in material waste, and the particle size requirements of battery-grade lithium carbonate cannot be met. If the particle size D50 is too large, the sulfate cannot be released well, resulting in the inability to fully wash away the sulfate, and the particle size requirements of battery-grade lithium carbonate cannot be met.

[0030] The method for removing sulfate from battery-grade lithium carbonate provided by the present invention comprises the following steps: after the sulfate impurities are roughly removed from the lithium carbonate, the lithium carbonate is ground to a particle size D50 of 4 μm-7 μm, so that the coated sulfate can be fully released, and after washing, the sulfate content is greatly reduced; the method of the present invention is not only simple in process and easy to operate, but also can efficiently reduce the sulfate content in the battery-grade lithium carbonate, effectively improve the quality of the lithium carbonate product, and is suitable for industrial production and application.

[0031] In the present invention, lithium carbonate includes but is not limited to lithium carbonate (Li2CO3) products generated by lithium precipitation, for example, it can be a lithium carbonate (Li2CO3) product obtained by lithium precipitation reaction of sodium carbonate (Na2CO3) and lithium sulfate (Li2SO4), and the reaction formula is Na2CO3+Li2SO4→Li2CO3↓+Na2SO4.

[0032] In a preferred embodiment, the washing method includes but is not limited to stirring and washing with water, and the solid content of the finely ground material during washing is ≤70%. The solid content of the material can be, for example, 50%, 55%, 60%, 65%, 70%, but is not limited to this, which is more conducive to further removing sulfate and significantly reducing the sulfate content.

[0033] In a preferred embodiment, during the washing process, the stirring speed can be 100r / min-120r / min, and the stirring time can be 10min-20min. Appropriate stirring speed and time are more conducive to further improving the removal effect of sulfate and further reducing the sulfate content.

[0034] In a preferred embodiment, the insulation temperature during the washing process can be above 95° C., which is more conducive to further improving the removal effect of sulfate and can ensure that the sulfate content is effectively reduced.

[0035] In a preferred embodiment, the solid-liquid separation method includes but is not limited to separation by centrifugation, which is more conducive to further improving the separation effect of lithium carbonate.

[0036] In a preferred embodiment, during the centrifugation process, the centrifugal speed can be 1250r / min-1470r / min, and the centrifugal time can be 720s. Appropriate centrifugal speed and time are more conducive to ensuring sufficient separation to obtain the lithium carbonate product.

[0037] In the present invention, after the solid-liquid separation, the step of drying the washed material is also included to control the water content in the lithium carbonate.

[0038] In the present invention, the lithium carbonate from which impurities have been roughly removed is finely ground to a particle size D50 of 4 μm-7 μm, and then stirred and washed with water, and then centrifuged. With the coordinated cooperation of each step and its process parameters, the sulfate content is effectively reduced, and the influence of sulfate peritectic caused by the lithium precipitation process is greatly improved, thereby achieving the purpose of improving the quality of lithium carbonate products through simple process adjustments.

[0039] It should be emphasized that when the sulfate content exceeds the standard of 850ppm due to peritectic formation, the sulfate content of lithium carbonate can be reduced to 630ppm by fine grinding and then stirring and washing; when the sulfate content is 660ppm, the sulfate content of lithium carbonate can be reduced to 500ppm by fine grinding and then stirring and washing; it can be seen that the present invention solves the technical problem that it is difficult to effectively reduce the sulfate content in battery-grade lithium carbonate products in the prior art.

[0040] According to a second aspect of the present invention, there is provided an application of any of the methods described above in a lithium carbonate production process.

[0041] The application of the method for removing sulfate from battery-grade lithium carbonate provided by the present invention is beneficial to improving the quality of battery-grade lithium carbonate products.

[0042] A typical production process of battery-grade lithium carbonate, see the flow chart Figure 1 , including the following steps:

[0043] (a) subjecting lithium sulfate and sodium carbonate to lithium precipitation reaction in a solution, and centrifuging to obtain a crude lithium carbonate product;

[0044] (b) stirring and washing the crude lithium carbonate obtained in step (a) to roughly remove sulfate impurities, centrifuging, and drying to obtain lithium carbonate after roughly removing impurities;

[0045] (c) finely grinding the lithium carbonate obtained in step (b) after rough impurity removal to a particle size D50 of 4 μm-7 μm to ensure that the sulfate ions coated in the reaction in step (a) are fully released to obtain a finely ground material;

[0046] (d) adding water to the finely ground material obtained in step (c), stirring and washing, centrifuging, and drying in a drying kiln to obtain a final lithium carbonate product;

[0047] The washing water can be recycled to prepare the alkali solution in step (a), or recycled to perform stirring washing in step (b).

[0048] When the sulfate content exceeds the standard and reaches 850ppm due to peritectic, the sulfate content of lithium carbonate can be reduced to 630ppm by fine grinding and stirring and washing; when the sulfate content is 660ppm, the sulfate content of lithium carbonate can be reduced to 500ppm by fine grinding and stirring and washing; in short, regardless of whether the sulfate content in the product obtained by the traditional lithium carbonate production process meets the standard, lithium carbonate can be effectively reduced by fine grinding and stirring and washing, thereby greatly improving the quality of battery-grade lithium carbonate. The main content of the obtained battery-grade lithium carbonate is ≥99.5%, and the sulfate content is ≤650ppm. The other indicators meet the standard requirements of battery-grade lithium carbonate in YS / T582-2023.

[0049] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0050] Example 1

[0051] A method for removing sulfate from battery-grade lithium carbonate comprises the following steps:

[0052] S1: adding water to the crude lithium carbonate, stirring and washing to roughly remove sulfate impurities, centrifuging and drying to obtain lithium carbonate after roughly removing impurities, wherein the sulfate content is 750 ppm;

[0053] Wherein, crude lithium carbonate is obtained by lithium sulfate and sodium carbonate precipitation reaction;

[0054] S2: finely grinding the lithium carbonate after rough impurity removal to a particle size D50 of 4 μm to obtain a finely ground material;

[0055] S3: Put the finely ground material into a stirring and washing kettle, add water for stirring and washing (temperature ≥ 95°C), and control the solid content of the material in the stirring and washing kettle to be 50%;

[0056] Among them, the stirring speed is 100r / min and the stirring time is 15min;

[0057] S4: The materials in the kettle are centrifuged and the solid materials are dried in a drying kiln and then transported to the packaging room for packaging to obtain a battery-grade lithium carbonate product with a sulfate content of 600ppm.

[0058] Example 2

[0059] The difference between this embodiment and embodiment 1 is that in step S2, the material is finely ground to a particle size D50 of 5 μm;

[0060] The remaining steps and process parameters are the same as those in Example 1, and a battery-grade lithium carbonate product is obtained, and its sulfate content is 610 ppm.

[0061] Example 3

[0062] The difference between this embodiment and embodiment 1 is that in step S2, the material is finely ground to a particle size D50 of 6 μm;

[0063] The remaining steps and process parameters are the same as those in Example 1, and a battery-grade lithium carbonate product is obtained, and its sulfate content is 630 ppm.

[0064] Example 4

[0065] The difference between this embodiment and embodiment 1 is that in step S2, the material is finely ground to a particle size D50 of 7 μm;

[0066] The remaining steps and process parameters are the same as those in Example 1, and a battery-grade lithium carbonate product is obtained, and its sulfate content is 660 ppm.

[0067] Example 5

[0068] The difference between this embodiment and embodiment 1 is that in step S3, the solid content of the material in the stirring and washing kettle is controlled to be 60%;

[0069] The remaining steps and process parameters are the same as those in Example 1 to obtain a battery-grade lithium carbonate product with a sulfate content of 600 ppm.

[0070] Example 6

[0071] The difference between this embodiment and embodiment 1 is that in step S3, the solid content of the material in the stirring and washing kettle is controlled to be 70%;

[0072] The remaining steps and process parameters are the same as those in Example 1, and a battery-grade lithium carbonate product is obtained, and its sulfate content is 630 ppm.

[0073] Example 7

[0074] The difference between this embodiment and embodiment 1 is that in step S3, the solid content of the material in the stirring and washing kettle is controlled to be 80%;

[0075] The remaining steps and process parameters are the same as those in Example 1, and a battery-grade lithium carbonate product is obtained, and its sulfate content is 650 ppm.

[0076] Example 8

[0077] The difference between this embodiment and embodiment 1 is that in step S3, the stirring speed is 110 r / min and the stirring time is 15 min;

[0078] The remaining steps and process parameters are the same as those in Example 1 to obtain a battery-grade lithium carbonate product with a sulfate content of 600 ppm.

[0079] Example 9

[0080] The difference between this embodiment and embodiment 1 is that in step S3, the stirring speed is 120 r / min and the stirring time is 15 min;

[0081] The remaining steps and process parameters are the same as those in Example 1, and a battery-grade lithium carbonate product is obtained, and its sulfate content is 590 ppm.

[0082] Comparative Example 1

[0083] The difference between this comparative example and Example 1 is that in step S1, sulfate impurities are not roughly removed;

[0084] The remaining steps and process parameters are the same as those in Example 1, and a battery-grade lithium carbonate product is obtained, and its sulfate content is 670 ppm.

[0085] Compared with Example 1, the defect of this comparative example is that, since the initial sulfate concentration is relatively high, it is necessary to reduce the agitation concentration for washing, which will affect the production efficiency and wash water balance in actual production.

[0086] Comparative Example 2

[0087] The difference between this comparative example and Example 1 is that in step S2, the material is finely ground to a particle size D50 of 2 μm;

[0088] The remaining steps and process parameters are the same as those in Example 1, and a battery-grade lithium carbonate product is obtained, and its sulfate content is 530 ppm.

[0089] Compared with Example 1, the defect of this comparative example is that, since the material particles are too fine, they are easily filtered during centrifugation, resulting in material waste, and at the same time, the particle size requirements of battery-grade lithium carbonate products cannot be met.

[0090] Comparative Example 3

[0091] The difference between this comparative example and Example 1 is that in step S2, the material is finely ground to a particle size D50 of 9 μm;

[0092] The remaining steps and process parameters are the same as those in Example 1, and a battery-grade lithium carbonate product is obtained, and its sulfate content is 680 ppm.

[0093] Compared with Example 1, the defect of this comparative example is that, since the sulfate ions coated in the lithium carbonate cannot be well released, the sulfate ions cannot be fully washed away, and the particle size requirements of battery-grade lithium carbonate products cannot be met.

[0094] It can be seen that the method for removing sulfate from battery-grade lithium carbonate of the present invention is that the lithium carbonate from which impurities are roughly removed is finely ground to a particle size D50 of 4μm-7μm, then stirred and washed with water, and then centrifuged. With the coordinated cooperation of each step and its process parameters, the sulfate content can be effectively reduced, the influence of sulfate peritectic caused by the lithium precipitation process is greatly improved, and it is beneficial to improve the quality of battery-grade lithium carbonate products.

[0095] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for removing sulfate from battery-grade lithium carbonate, characterized in that: The following steps are involved: The lithium carbonate is roughly ground to a particle size D50 of 4 μm-7 μm after sulfate impurities are removed to obtain a finely ground material, and the finely ground material is washed and solid-liquid separated to obtain the battery-grade lithium carbonate.

2. The method according to claim 1, characterized in that: The lithium carbonate includes lithium carbonate generated by lithium precipitation.

3. The method according to claim 2, characterized in that The lithium carbonate is obtained by reacting sodium carbonate with lithium sulfate to precipitate lithium.

4. The method according to any one of claims 1 to 3, characterized in that: The washing method includes stirring washing with water.

5. The method according to claim 4, characterized in that The solid content of the finely ground material during washing is ≤70%.

6. The method according to claim 5, characterized in that The stirring speed of the washing is 100r / min-120r / min, and the stirring time of the washing is 10min-20min; Preferably, the reaction temperature of the washing is ≥95°C.

7. The method according to any one of claims 1 to 3, characterized in that: The solid-liquid separation method includes separation by centrifugation.

8. The method according to claim 7, characterized in that The centrifugal speed is 1250r / min-1470r / min.

9. The method according to claim 7, characterized in that: After the solid-liquid separation, the method further comprises the step of drying the washed material.

10. Use of the method according to any one of claims 1 to 9 in the production of lithium carbonate.