Method for preparing multi-morphology anhydrous magnesium carbonate by inducing solid-phase conversion of magnesite through template agent
Through the solid phase conversion method induced by template agent, the problems of unsatisfactory morphology and high production costs of anhydrous magnesium carbonate products were solved, and the preparation of anhydrous magnesium carbonate with uniform particle size, regular morphology and good dispersion were achieved. Its application areas and reduces production costs.
Patent Information
- Application Number
- CN202410975425.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-22
AI Technical Summary
The existing technology is difficult to industrialize the production of efficient and low-cost anhydrous magnesium carbonate on a large scale. The product has poor morphology, uneven particle size distribution, and problems with by-products and environmental pollution, which limits its application potential.
The solid phase conversion method induced by template agents is used, natural magnesite and salicylic acid are used as raw materials, and EDTA or its sodium salt is introduced as template agents. Multi-morphological anhydrous magnesium carbonate is prepared through solid phase conversion method, and the process flow is simplified. Reduced costs, control particle size and morphology.
The particle size distribution of anhydrous magnesium carbonate is achieved, the morphology is regular and the dispersion is good, the process flow is simplified, the production cost is reduced, the application field is broadened, and the industrial application prospects are good.
Smart Images

Figure CN118993119A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemical synthesis methods, and in particular to a method for preparing multi-morphological anhydrous magnesium carbonate by inducing solid-phase transformation of magnesite with a template. Background Art
[0002] Anhydrous magnesium carbonate (MgCO3) is a single crystal of magnesium carbonate salt. It exists in the form of magnesite in nature. It has the characteristics of low price, non-toxicity, good biocompatibility, etc. It is an important inorganic chemical material and is widely used in plastics, papermaking, coatings, ceramics, medicine and other industries.
[0003] In recent years, anhydrous magnesium carbonate has attracted the attention of many researchers as a new type of inorganic flame retardant. Compared with traditional organic halogen flame retardants, it has the advantages of being non-toxic, non-corrosive, and environmentally friendly. At the same time, compared with inorganic halogen-free flame retardants such as aluminum hydroxide and magnesium hydroxide, anhydrous magnesium carbonate not only has the advantages of fast thermal decomposition speed, heat absorption and cooling, and large heat absorption heat capacity, but also can decompose and release a large amount of carbon dioxide to isolate the air, playing an effective fire extinguishing role. Its heat loss weight is as high as 52.2%, which is much higher than the currently widely used aluminum hydroxide (34.6%) and magnesium hydroxide (30.9%). Therefore, anhydrous magnesium carbonate is the best flame retardant material reported so far.
[0004] However, all magnesium carbonate products on the market, except for natural magnesite, are hydrated magnesium carbonate, and there is almost no ready-made anhydrous magnesium carbonate product for sale. 2+ and Mn 2+ In addition to the fact that impurities such as magnesium sulfate have almost no contribution to flame retardancy, the natural magnesite powder after mechanical grinding has shortcomings such as uneven particle size, irregular morphology and uncontrollable shape, which leads to the flame retardant efficiency of magnesite being much lower than that of anhydrous magnesium carbonate flame retardant.
[0005] Therefore, the synthesis of anhydrous magnesium carbonate with uniform particle size distribution, good dispersibility and regular morphology will significantly improve its high-efficiency, high-value and high-quality comprehensive utilization, which is of great significance. Therefore, the preparation of anhydrous magnesium carbonate has received great attention. The research on anhydrous magnesium carbonate is currently in its infancy. Although there have been reports of the successful synthesis of anhydrous magnesium carbonate materials, overall, the morphology of the prepared products is not ideal, and most of the products have the disadvantages of uneven particle size distribution and poor dispersibility; worthless by-products are often produced during the reaction, which is not conducive to improving product purity; the process is complex and the environment is harsh; the raw materials for preparation are mostly analytically pure chemical reagents, which have problems such as high synthesis cost and by-products that easily cause environmental pollution. It is difficult to industrialize large-scale production, which is not conducive to the exploration of material applications in the next stage. Summary of the invention
[0006] In view of the shortcomings of the current prior art, the present invention provides a method for preparing anhydrous magnesium carbonate with multiple morphologies by using a template-induced solid-phase transformation of magnesite. The method uses natural magnesite as a magnesium source, salicylic acid as a carbon source, and EDTA or one of its sodium salts as a template, and adopts a solid-phase transformation method to prepare anhydrous magnesium carbonate crystals. The method has the advantages of simple process flow, low production cost, and the prepared anhydrous magnesium carbonate has uniform particle size distribution, good dispersibility, and regular morphology.
[0007] The technical solutions adopted to achieve the above objectives are:
[0008] A method for preparing multi-morphological anhydrous magnesium carbonate by template-induced solid phase transformation of magnesite is as follows:
[0009] (1) Prepare a salicylic acid solution, add magnesite to the salicylic acid solution, and stir to obtain a mixed solution.
[0010] (2) placing the mixed solution obtained in step (1) in a reaction kettle, heating and stirring, and after the reaction is completed, naturally cooling to room temperature, filtering, washing, and drying to obtain anhydrous magnesium carbonate crystals.
[0011] Furthermore, the solvent of the salicylic acid solution in step (1) is a mixture of deionized water and anhydrous ethanol; the concentration of the salicylic acid solution is 0.05-0.85 mol / L, the amount of magnesite is 5-85 mg / mL, and the stirring rate is 100-500 r / min.
[0012] Furthermore, in the solvent of the salicylic acid solution, the volume ratio of deionized water to anhydrous ethanol is 1:(1-1.1).
[0013] Furthermore, in the step (2), the reaction temperature is 120-240° C., the reaction time is 2-16 h, and the reaction stirring rate is 100-600 r / min.
[0014] Furthermore, the step (1) of the method for preparing polymorphic anhydrous magnesium carbonate by using a template to induce solid phase transformation of magnesite also includes a template.
[0015] Furthermore, the template agent is EDTA or one of its sodium salts.
[0016] Furthermore, the amount of the template agent is 2.5-35% of the total mass of salicylic acid and magnesite in the mixed solution.
[0017] The invention provides a multi-morphology anhydrous magnesium carbonate, wherein the multi-morphology anhydrous magnesium carbonate has a pure phase block or a pure phase rod morphology.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] First, the present invention directly uses magnesite as raw material, which is rich in source and low in cost, and is an excellent raw material choice, and can replace chemical reagents such as magnesium sulfate, magnesium chloride, magnesium nitrate, and magnesium hydroxide.
[0020] Second: The present invention is the first to use the solid-phase conversion method to directly transform dolomite into pure-phase anhydrous magnesium carbonate. The process is simple and the cycle is short. In addition, anhydrous magnesium carbonate crystals with uniform particle size distribution, regular morphology and good dispersibility can be obtained in a short time, which has good industrial application prospects.
[0021] Third: The present invention can effectively improve and control the morphology and particle size of anhydrous magnesium carbonate by introducing a template to obtain anhydrous magnesium carbonate crystals with different morphologies and particle size distributions, thereby broadening the application field of anhydrous magnesium carbonate. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The XRD pattern of the anhydrous magnesium carbonate crystals prepared in Example 1-6;
[0023] Figure 2 The particle size distribution diagram of the anhydrous magnesium carbonate crystals prepared in Examples 1-6;
[0024] Figure 3 The SEM image of the anhydrous magnesium carbonate prepared in Example 1; the upper right corner is a high-magnification SEM image;
[0025] Figure 4 The SEM image of anhydrous magnesium carbonate prepared in Example 2; the upper right corner is a high-magnification SEM image;
[0026] Figure 5 The SEM image of anhydrous magnesium carbonate prepared in Example 5; the upper right corner is a high-magnification SEM image;
[0027] Figure 6 This is a SEM image of anhydrous magnesium carbonate prepared in Example 6; the upper right corner is a high-magnification SEM image. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments.
[0029] The following provides a specific implementation of a method for preparing anhydrous magnesium carbonate with multiple morphologies by template-induced solid-phase transformation of magnesite, which is divided into a method for preparing anhydrous magnesium carbonate by solid-phase transformation of magnesite and a method for preparing anhydrous magnesium carbonate by template-mediated solid-phase transformation of magnesite.
[0030] A method for preparing multi-morphological anhydrous magnesium carbonate by template-induced solid-phase transformation of magnesite, comprising the following steps:
[0031] Embodiment 1:
[0032] Prepare 0.25 mol / L salicylic acid solution with a volume ratio of deionized water and anhydrous ethanol of 1:1, add magnesite in an amount of 30 mg / mL, and the magnetic stirring rate is 100 r / min. Add the raw materials into the reactor device, the reaction temperature is 180°C, the reaction time is 9 hours, and the reaction stirring rate is 200 r / min. After the reactor is naturally cooled to room temperature, the mixture is centrifuged and filtered to obtain a filter cake, which is dried in an oven at 60°C for 8 hours to obtain pure phase anhydrous magnesium carbonate crystals. Figure 1 , Figure 2 and Figure 3 It can be seen that the obtained product is a pure phase block anhydrous magnesium carbonate crystal with a diameter of 30 to 80 μm and an average particle size of 60 μm.
[0033] Embodiment 2:
[0034] Prepare 0.55 mol / L salicylic acid solution with a volume ratio of deionized water and anhydrous ethanol of 1:1, add magnesite in an amount of 50 mg / mL, and the magnetic stirring rate is 100 r / min. Add the raw materials into the reactor device, the reaction temperature is 180°C, the reaction time is 12h, and the reaction stirring rate is 400 r / min. After the reactor is naturally cooled to room temperature, the mixture is centrifuged and filtered to obtain a filter cake, which is dried in an oven at 60°C for 12h to obtain pure phase anhydrous magnesium carbonate crystals. Figure 1 , Figure 2 and Figure 4 It can be seen that the obtained product is a pure phase block anhydrous magnesium carbonate crystal with a diameter of 20 to 80 μm and an average particle size of 47 μm.
[0035] Embodiment 3:
[0036] A 0.55 mol / L salicylic acid solution was prepared with a volume ratio of deionized water and anhydrous ethanol of 1:1, and magnesite was added in an amount of 70 mg / mL. The magnetic stirring rate was 100 r / min, and the raw materials were added to a reactor device. The reaction temperature was 180°C, the reaction time was 12 h, and the reaction stirring rate was 400 r / min. After the reactor was naturally cooled to room temperature, the mixture was centrifuged and filtered to obtain a filter cake, which was dried in an oven at 60°C for 12 h to obtain pure phase anhydrous magnesium carbonate crystals.
[0037] Embodiment 4:
[0038] A 0.15 mol / L salicylic acid solution was prepared with a volume ratio of deionized water and anhydrous ethanol of 1:1, and magnesite was added in an amount of 10 mg / mL. The magnetic stirring rate was 100 r / min, and the raw materials were added to a reactor device. The reaction temperature was 180°C, the reaction time was 10 h, and the reaction stirring rate was 100 r / min. After the reactor was naturally cooled to room temperature, the mixture was centrifuged and filtered to obtain a filter cake, which was dried in an oven at 60°C for 12 h to obtain pure phase anhydrous magnesium carbonate crystals.
[0039] Embodiment 5:
[0040] Prepare 0.55 mol / L salicylic acid solution with a volume ratio of deionized water and anhydrous ethanol of 1:1, add magnesite in an amount of 50 mg / mL, add 5% of the total mass of the reactants, disodium EDTA, and stir at a magnetic rate of 200 r / min. Add the raw materials to the reactor device, the reaction temperature is 180°C, the reaction time is 12h, the reaction stirring rate is 400 r / min, and after the reactor is naturally cooled to room temperature, the mixture is centrifuged and filtered to obtain a filter cake, which is dried in an oven at 60°C for 12h to obtain pure anhydrous magnesium carbonate crystals. Figure 1 , Figure 2 and Figure 5 It can be seen that the obtained product is a pure phase rod-shaped anhydrous magnesium carbonate crystal with a length of 20 to 50 μm, a width of 10 to 20 μm and an average particle size of 37 μm.
[0041] Embodiment 6:
[0042] Prepare 0.55 mol / L salicylic acid solution with a volume ratio of 1:1 between deionized water and anhydrous ethanol, add magnesite in an amount of 50 mg / mL, add EDTA disodium at a total mass of 15% of salicylic acid and magnesite, and stir at a magnetic rate of 300 r / min. Add the raw materials to the reactor device, the reaction temperature is 180°C, the reaction time is 12h, the reaction stirring rate is 400 r / min, and after the reactor is naturally cooled to room temperature, the mixture is centrifuged and filtered to obtain a filter cake, which is dried in an oven at 60°C for 12h to obtain pure phase anhydrous magnesium carbonate crystals. Figure 1 , Figure 2 and Figure 6 It can be seen that the obtained product is a pure phase rod-shaped anhydrous magnesium carbonate crystal with a length of 20 to 50 μm, a width of 10 to 20 μm and an average particle size of 37 μm.
[0043] Embodiment 7:
[0044] 0.25 mol / L salicylic acid solution was prepared with a volume ratio of deionized water and anhydrous ethanol of 1:1, and magnesite was added in an amount of 40 mg / mL, and 3% of the total mass of salicylic acid and magnesite was added. The magnetic stirring rate was 100 r / min, and the raw materials were added to the reactor device. The reaction temperature was 150°C, the reaction time was 8 hours, and the reaction stirring rate was 200 r / min. After the reactor was naturally cooled to room temperature, the mixture was centrifuged and filtered to obtain a filter cake, which was dried in an oven at 60°C for 12 hours to obtain pure phase anhydrous magnesium carbonate crystals.
[0045] Embodiment 8:
[0046] A 0.15 mol / L salicylic acid solution was prepared with a volume ratio of deionized water and anhydrous ethanol of 1:1, and magnesite was added in an amount of 10 mg / mL, and 25% of the total mass of salicylic acid and magnesite was added with disodium EDTA. The magnetic stirring rate was 400 r / min, and the raw materials were added to a reactor device. The reaction temperature was 200°C, the reaction time was 10 h, and the reaction stirring rate was 100 r / min. After the reactor was naturally cooled to room temperature, the mixture was centrifuged and filtered to obtain a filter cake, which was dried in an oven at 60°C for 12 h to obtain pure phase anhydrous magnesium carbonate crystals.
[0047] As can be seen from the above embodiments, in the process of preparing anhydrous magnesium carbonate crystals, the present invention can directly convert natural dolomite into pure phase anhydrous magnesium carbonate crystals by solid phase conversion method; adding an appropriate amount of EDTA or its sodium salt as a template agent can regulate the morphology and size of anhydrous magnesium carbonate. The present invention not only has a simple process flow and low synthesis cost, but also has great industrialization potential, and the obtained anhydrous magnesium carbonate particles have uniform size, good dispersibility, regular and diverse morphology, and can be used as a high-quality powder filler in the field of inorganic chemical industry.
[0048] The above is only a preferred embodiment of the present invention, and should not limit the scope of the present invention. All equivalent changes and modifications made according to the scope of this application should still fall within the scope of the present invention. In the following specific implementations, the raw materials used are purchased from the market and used directly without treatment.
Claims
1. A method for preparing anhydrous magnesium carbonate with multiple morphologies by template-induced solid phase transformation of magnesite, characterized in that: The following steps are included: (1) preparing a salicylic acid solution, adding magnesite to the salicylic acid solution, and stirring to obtain a mixed solution; (2) placing the mixed solution obtained in step (1) in a reaction kettle, heating and stirring, and after the reaction is completed, naturally cooling to room temperature, filtering, washing, and drying to obtain anhydrous magnesium carbonate crystals.
2. The method for preparing polymorphic anhydrous magnesium carbonate by template-induced solid phase transformation of magnesite according to claim 1, characterized in that: The solvent of the salicylic acid solution in step (1) is a mixture of deionized water and anhydrous ethanol; the concentration of the salicylic acid solution is 0.05-0.85 mol / L, the amount of magnesite is 5-85 mg / mL, and the stirring rate is 100-500 r / min.
3. The method for preparing multi-morphological anhydrous magnesium carbonate by template-induced solid phase transformation of magnesite according to claim 2, characterized in that: In the solvent of the salicylic acid solution, the volume ratio of deionized water to anhydrous ethanol is 1:(1-1.1).
4. The method for preparing multi-morphological anhydrous magnesium carbonate by template-induced solid phase transformation of magnesite according to claim 1, characterized in that: In the step (2), the reaction temperature is 120-240° C., the reaction time is 2-16 h, and the reaction stirring rate is 100-600 r / min.
5. The method for preparing multi-morphological anhydrous magnesium carbonate by template-induced solid phase transformation of magnesite according to claim 1, characterized in that: The step (1) also includes adding a template.
6. The method for preparing multi-morphological anhydrous magnesium carbonate by template-induced solid phase transformation of magnesite according to claim 5, characterized in that: The template agent is EDTA or one of its sodium salts.
7. The method for preparing multi-morphological anhydrous magnesium carbonate by template-induced solid phase transformation of magnesite according to claim 6, characterized in that: The dosage of the template agent is 2.5-35% of the total mass of salicylic acid and magnesite in the mixed solution.
8. A polymorphic anhydrous magnesium carbonate, characterized in that: The polymorphic anhydrous magnesium carbonate is prepared by the method for preparing polymorphic anhydrous magnesium carbonate by template-induced solid phase transformation of magnesite as described in any one of claims 1 to 7.