Tempered glass composition as well as preparation method and application thereof

By using specific proportions of inorganic potassium salt and organic potassium salt compositions for chemical strengthening of glass, the problem of insufficient strength and warping of the intermediate layer of hollow glass is solved, and an efficient and environmentally friendly glass strengthening process is realized, which improves the mechanical properties of glass and Security.

CN118993559AActive Publication Date: 2024-11-22QINHUANGDAO GLASS IND RES & DESIGN INST
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411078705.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

In the prior art, the intermediate layer of hollow glass has a small strength and is prone to warping after chemical reinforcement treatment, which affects its mechanical properties and safety of use.

Method used

Chemical strengthening of the glass is carried out by solvent method, molten salt or slurry method, including inorganic potassium salt and organic potassium salt, with a specific molar ratio of potassium sulfite, potassium hydroxide and potassium sorbate. Control temperature and drying conditions to reduce warping and increase the strength of the glass.

Benefits of technology

It effectively improves the strength of the glass, reduces warping, reduces energy consumption and production costs, and has a simple and environmentally friendly process, and does not produce harmful substances. It is suitable for strengthening large-area glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993559A_ABST
    Figure CN118993559A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of glass, in particular to a tempered glass composition as well as a preparation method and application thereof. The tempered glass composition comprises inorganic potassium salt and organic potassium salt, wherein the molar ratio of the inorganic potassium salt to the organic potassium salt is (1-3): (1-2); the inorganic potassium salt is selected from at least one of potassium nitrate, potassium chloride, potassium sulfate, potassium sulfite, potassium phosphate, dipotassium phosphate, monopotassium phosphate and potassium hydroxide; the organic potassium salt is selected from at least one of potassium benzoate, potassium citrate and potassium sorbate. The toughened glass composition provided by the invention comprises specific organic potassium salt and inorganic potassium salt in a specific proportion, and when the toughened glass composition is used for glass reinforcement, the warping phenomenon of glass is remarkably improved, and meanwhile, the strength of the glass is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of glass, and in particular to a tempered glass composition and a preparation method and application thereof. Background Art

[0002] The external structure is the key part of green building energy-saving technology, while doors and windows are the weak links in building energy-saving. As a building energy-saving material, hollow glass is widely used because of its good heat insulation and sound insulation performance. In order to ensure the safe use of hollow glass, the flat glass used to make hollow glass needs to have certain mechanical strength and other properties. However, the strength of ordinary flat glass produced by the float process is relatively low (generally 20-40MPa), and it cannot be directly used to make hollow glass. It needs to be strengthened and reach a certain strength before it can be used. For three-glass two-cavity and more multi-cavity hollow glass, the middle layer of glass needs to have a certain load impact resistance. Therefore, thin glass (thickness ≤ 2mm) needs to be strengthened to improve its physical and mechanical properties before it can be used as middle layer glass.

[0003] Chemical strengthening technology, also known as ion exchange technology, is widely used in construction, transportation, industry and other fields because it can form a compressive stress layer on the surface of glass to improve the mechanical strength of glass. The chemical strengthening process not only directly affects the performance of chemically strengthened glass, but also determines the energy consumption and cost of the strengthening process. Conventional ion exchange method uses potassium nitrate as molten salt, in which K + Ions can be completely ionized, and ion exchange can be quickly carried out by immersing glass in molten salt. The middle layer of insulating glass uses thin glass, and this method is used to chemically strengthen the thin glass. Due to the different strengths formed on the upper and lower surfaces of the glass after chemical strengthening, the glass will warp.

[0004] Therefore, in view of the problem that the intermediate layer glass used to prepare insulating glass in the prior art has low strength and the glass warps after chemical strengthening treatment, it is necessary to study the glass strengthening process. Summary of the invention

[0005] In view of the problems in the prior art that the intermediate layer glass of insulating glass has low strength and that the glass warps after chemical strengthening treatment, the present invention provides a strengthened glass composition and a preparation method and application thereof.

[0006] To achieve the above technical objectives, the present invention provides a strengthened glass composition, comprising an inorganic potassium salt and an organic potassium salt, wherein the molar ratio of the inorganic potassium salt to the organic potassium salt is 1-3:1-2;

[0007] The inorganic potassium salt is selected from at least one of potassium nitrate, potassium chloride, potassium sulfate, potassium sulfite, potassium phosphate, dipotassium hydrogen phosphate, potassium dihydrogen phosphate, and potassium hydroxide;

[0008] The organic potassium salt is selected from at least one of potassium benzoate, potassium citrate and potassium sorbate.

[0009] Furthermore, the strengthened glass composition comprises potassium sulfite, potassium hydroxide and potassium sorbate; preferably, the molar ratio of potassium sulfite, potassium hydroxide and potassium sorbate is 0.5-1:0.5-1:2.

[0010] The present invention also provides a method for preparing the above-mentioned strengthened glass composition, which comprises taking an organic potassium salt and an inorganic potassium salt according to the above-mentioned molar ratio, and mixing them to obtain the strengthened glass composition.

[0011] The present invention also provides an application of the above-mentioned strengthened glass composition or the strengthened glass composition prepared by the preparation method of the above-mentioned strengthened glass composition in glass strengthening.

[0012] The present invention also provides a chemical strengthening process for glass, which uses a solvent method, a molten salt method or a slurry method to strengthen the glass;

[0013] The solvent method comprises mixing the above-mentioned strengthened glass composition or the strengthened glass composition obtained by the preparation method of the above-mentioned strengthened glass composition with solvent 1 to obtain a mixture, and then coating the mixture on the glass surface and drying to obtain the strengthened glass;

[0014] The molten salt method comprises heating the above-mentioned strengthened glass composition or the strengthened glass composition prepared by the above-mentioned preparation method of the strengthened glass composition to obtain molten salt, coating the molten salt on the surface of the glass, and drying to obtain the strengthened glass;

[0015] The slurry method comprises mixing the above-mentioned strengthened glass composition or the strengthened glass composition prepared by the above-mentioned preparation method of the strengthened glass composition with a solvent 2 and a binder to prepare a mixture, coating the mixture on a glass surface, and drying to obtain the strengthened glass.

[0016] Furthermore, in the solvent method, the solvent 1 is selected from water and / or ethanol; and / or the ratio of the volume of the solvent 1 to the mole of the tempered glass composition is 100-700 mL:2-4 mol; and / or the drying step comprises first drying at a temperature of 80-170° C. for 5-25 min, then heating the temperature to 220-300° C. at a heating rate of 10-30° C. / min, and keeping the temperature at 220-300° C. for 20-60 min.

[0017] Furthermore, in the slurry method, the binder is selected from clay and / or diatomaceous earth; and / or, the solvent 2 is selected from water and / or ethanol; and / or, the ratio of the mole of the tempered glass composition, the volume of the solvent 2 and the mass of the binder is 2-4 mol:100-700 mL:50-200 g; and / or, the drying step comprises first drying at a temperature of 50-100°C for 20-50 min, then heating the temperature to 150-250°C at a heating rate of 8-25°C / min, and keeping the temperature at 150-250°C for 60-120 min.

[0018] Furthermore, in the molten salt method, the heating temperature is 240-430°C; and / or the drying step includes first drying at a temperature of 80-170°C for 5-20 minutes, then heating the temperature to 220-300°C at a heating rate of 5-20°C / min, and keeping warm at 220-300°C for 20-60 minutes.

[0019] Furthermore, the coating method in the solvent method, molten salt method or slurry method is selected from at least one of brushing, printing and spraying; and / or, the solvent method, molten salt method or slurry method also includes cooling and cleaning steps after drying.

[0020] The technical solution of the present invention has the following beneficial effects:

[0021] (1) The present invention provides a tempered glass composition, comprising an inorganic potassium salt and an organic potassium salt, wherein the molar ratio of the inorganic potassium salt to the organic potassium salt is 1-3:1-2; the inorganic potassium salt is selected from at least one of potassium nitrate, potassium chloride, potassium sulfate, potassium sulfite, potassium phosphate, dipotassium hydrogen phosphate, potassium dihydrogen phosphate, and potassium hydroxide; and the organic potassium salt is selected from at least one of potassium benzoate, potassium citrate, and potassium sorbate. The tempered glass composition provided by the present invention comprises specific organic potassium salts and inorganic potassium salts in specific proportions, and uses at least one of potassium benzoate, potassium citrate, and potassium sorbate as the organic potassium salt, and uses at least one of potassium nitrate, potassium chloride, potassium sulfate, potassium sulfite, potassium phosphate, dipotassium hydrogen phosphate, potassium dihydrogen phosphate, and potassium hydroxide as the inorganic potassium salt, so that the tempered glass composition is applied to the strengthening of glass, which can not only improve the warping phenomenon of the glass after strengthening, but also improve the strength of the glass. In the present invention, the K in the inorganic potassium salt is + The ions are easily ionized and then react with the Na + The present invention uses inorganic potassium salt with a low melting point to save energy. Secondly, the present invention uses organic potassium salt with a high melting point to prevent the organic potassium salt from being decomposed and volatilized by heat due to too low temperature during chemical strengthening. +Ions are not easy to ionize. When mixed with inorganic potassium salts, the K in the inorganic potassium salts is + Ions and Na in Glass + The ions are exchanged first. As the ion exchange proceeds, the K + ions enter the glass surface, and the K in the organic potassium salt + The ions are ionized and continue to react with Na + Ions are exchanged to strengthen the glass.

[0022] (2) The present invention provides a chemical strengthening process for glass, in which ion exchange is performed at a temperature of 300°C or below in a solvent method, a molten salt method or a slurry method. Since this temperature range is lower than the glass transition temperature, the ion exchange process can be carried out slowly, further reducing the glass warping phenomenon. Secondly, the chemical strengthening process in the present invention is simple, requires little investment, has low energy consumption, and has a flexible production method. When the glass is chemically strengthened, it is not necessary to immerse the glass in a solution to strengthen a large area of ​​glass with a size of 1.5m×2.0m or more. Finally, after the glass is chemically strengthened, the product generated on the surface of the glass is soluble in water or ethanol. The residue can be removed by washing the surface of the glass with deionized water or ethanol, which simplifies the chemical strengthening process and reduces production costs. The chemical strengthening process of the present invention does not produce harmful substances and does not harm the environment.

[0023] (3) The tempered glass composition provided by the present invention further improves the strength of the glass after chemical tempering by limiting the tempered glass composition to include potassium sulfite, potassium hydroxide and potassium sorbate. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 It is a schematic diagram of the structure of glass in the glass warpage test in Experimental Example 1 of the present invention.

[0026] Reference numerals:

[0027] h, the height of the arc; L, the length of the chord. DETAILED DESCRIPTION

[0028] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0029] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0030] Example 1

[0031] The present embodiment provides a tempered glass composition and a preparation method thereof, comprising taking 0.5 mol of potassium sulfite, 0.5 mol of potassium hydroxide and 2 mol of potassium sorbate respectively and mixing them according to a molar ratio of inorganic potassium salt to organic potassium salt of 1:2 to prepare a tempered glass composition.

[0032] This embodiment also provides a chemical strengthening process for glass, comprising: adding the above-mentioned strengthened glass composition to 600 mL of water, mixing to obtain a mixture, brushing the mixture on the surface of the glass and drying it at 120° C. for 20 minutes, then heating the temperature to 250° C. at a heating rate of 15° C. / min, keeping the temperature at 250° C. for 30 minutes, and washing the surface residue with water after natural cooling to obtain strengthened glass.

[0033] Example 2

[0034] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 1.

[0035] This embodiment also provides a chemical strengthening process for glass. The process parameters and methods are basically the same as those in Embodiment 1, except that "keeping at a temperature of 250° C. for 30 minutes" is replaced by "keeping at a temperature of 300° C. for 30 minutes".

[0036] Example 3

[0037] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 1.

[0038] This embodiment also provides a chemical strengthening process for glass. The process parameters and methods are basically the same as those in Embodiment 1, except that “keeping at a temperature of 250° C. for 30 minutes” is replaced by “keeping at a temperature of 250° C. for 60 minutes”.

[0039] Example 4

[0040] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 1.

[0041] This embodiment also provides a chemical strengthening process for glass. The process parameters and methods are basically the same as those in Embodiment 1, except that "keeping at a temperature of 250° C. for 30 minutes" is replaced by "keeping at a temperature of 300° C. for 60 minutes".

[0042] Example 5

[0043] The present embodiment provides a tempered glass composition and a preparation method thereof, comprising: taking 1 mol of potassium sulfite and 2 mol of potassium citrate respectively and mixing them according to a molar ratio of inorganic potassium salt to organic potassium salt of 1:2 to prepare a tempered glass composition.

[0044] This embodiment also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Embodiment 1.

[0045] Example 6

[0046] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 5.

[0047] This embodiment also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Embodiment 2.

[0048] Example 7

[0049] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 5.

[0050] This embodiment also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Embodiment 3.

[0051] Example 8

[0052] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 5.

[0053] This embodiment also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Embodiment 4.

[0054] Example 9

[0055] The present embodiment provides a tempered glass composition and a preparation method thereof, comprising: taking 1 mol of potassium sulfite, potassium citrate and potassium benzoate respectively and mixing them according to a molar ratio of inorganic potassium salt to organic potassium salt of 1:2 to prepare a tempered glass composition.

[0056] This embodiment also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Embodiment 1.

[0057] Example 10

[0058] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 9.

[0059] This embodiment also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Embodiment 2.

[0060] Embodiment 11

[0061] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 9.

[0062] This embodiment also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Embodiment 3.

[0063] Example 12

[0064] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 9.

[0065] This embodiment also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Embodiment 4.

[0066] Example 13

[0067] The present embodiment provides a tempered glass composition and a preparation method thereof, comprising: taking 0.6 mol of potassium sulfite, 1.2 mol of potassium hydroxide and 1.2 mol of potassium citrate respectively and mixing them according to a molar ratio of inorganic potassium salt to organic potassium salt of 3:2 to prepare a tempered glass composition.

[0068] This embodiment also provides a chemical strengthening process for glass, comprising: mixing the above-mentioned strengthened glass composition with 600 mL of water and 100 g of clay to obtain a mixture, brushing the mixture on a glass surface and drying it at 80° C. for 20 min, then heating the glass surface to 150° C. at a heating rate of 10° C. / min, keeping the temperature at 150° C. for 60 min, and washing the surface residue with water after natural cooling to obtain strengthened glass.

[0069] Embodiment 14

[0070] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 13.

[0071] This embodiment also provides a chemical strengthening process for glass. The process parameters and methods are basically the same as those in Embodiment 13, with the only difference being that “keeping at a temperature of 150° C. for 60 minutes” is replaced by “keeping at a temperature of 150° C. for 120 minutes”.

[0072] Embodiment 15

[0073] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 13.

[0074] This embodiment also provides a chemical strengthening process for glass. The process parameters and methods are basically the same as those in Embodiment 13, with the only difference being that “keeping at a temperature of 150° C. for 60 min” is replaced by “keeping at a temperature of 200° C. for 60 min”.

[0075] Example 16

[0076] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 13.

[0077] This embodiment also provides a chemical strengthening process for glass. The process parameters and methods are basically the same as those in Embodiment 13, with the only difference being that “keeping at a temperature of 150° C. for 60 minutes” is replaced by “keeping at a temperature of 200° C. for 120 minutes”.

[0078] Embodiment 17

[0079] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 13.

[0080] This embodiment also provides a chemical strengthening process for glass. The process parameters and methods are basically the same as those in Embodiment 13, with the only difference being that “keeping at a temperature of 150° C. for 60 minutes” is replaced by “keeping at a temperature of 250° C. for 60 minutes”.

[0081] Embodiment 18

[0082] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 13.

[0083] This embodiment also provides a chemical strengthening process for glass. The process parameters and methods are basically the same as those in Embodiment 13, with the only difference being that “keeping at a temperature of 150° C. for 60 minutes” is replaced by “keeping at a temperature of 250° C. for 120 minutes”.

[0084] Embodiment 19

[0085] This embodiment provides a strengthened glass composition and a preparation method thereof. The preparation method is the same as that of Embodiment 1.

[0086] This embodiment also provides a chemical strengthening process for glass, comprising: heating the above-mentioned strengthened glass composition at 350°C to obtain molten salt, applying the molten salt to the surface of the glass and drying it at 120°C for 20 minutes, then heating the temperature to 250°C at a heating rate of 10°C / min, keeping the temperature at 250°C for 30 minutes, cooling, and washing to obtain strengthened glass.

[0087] Comparative Example 1

[0088] This comparative example provides a strengthened glass composition, including 3 mol of potassium nitrate.

[0089] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 1.

[0090] Comparative Example 2

[0091] This comparative example provides a strengthened glass composition, and the strengthened glass composition is the same as that of comparative example 1.

[0092] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 2.

[0093] Comparative Example 3

[0094] This comparative example provides a strengthened glass composition, and the strengthened glass composition is the same as that of comparative example 1.

[0095] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 3.

[0096] Comparative Example 4

[0097] This comparative example provides a strengthened glass composition, and the strengthened glass composition is the same as that of comparative example 1.

[0098] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those of Example 4.

[0099] Comparative Example 5

[0100] This comparative example provides a strengthened glass composition, comprising taking 1.5 mol potassium nitrate and 1.5 mol potassium chloride and mixing them to prepare a strengthened glass composition.

[0101] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 1.

[0102] Comparative Example 6

[0103] This comparative example provides a strengthened glass composition. The strengthened glass composition is the same as that of comparative example 5.

[0104] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 2.

[0105] Comparative Example 7

[0106] This comparative example provides a strengthened glass composition. The strengthened glass composition is the same as that of comparative example 5.

[0107] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 3.

[0108] Comparative Example 8

[0109] This comparative example provides a strengthened glass composition. The strengthened glass composition is the same as that of comparative example 5.

[0110] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those of Example 4.

[0111] Comparative Example 9

[0112] This comparative example provides a strengthened glass composition, comprising taking 1.5 mol of potassium citrate and 1.5 mol of potassium benzoate and mixing them to prepare a strengthened glass composition.

[0113] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 1.

[0114] Comparative Example 10

[0115] This comparative example provides a strengthened glass composition. The strengthened glass composition is the same as that of comparative example 9.

[0116] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 2.

[0117] Comparative Example 11

[0118] This comparative example provides a strengthened glass composition. The strengthened glass composition is the same as that of comparative example 9.

[0119] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 3.

[0120] Comparative Example 12

[0121] This comparative example provides a strengthened glass composition. The strengthened glass composition is the same as that of comparative example 9.

[0122] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those of Example 4.

[0123] Comparative Example 13

[0124] This comparative example provides a tempered glass composition, comprising taking 1.5 mol of potassium sorbate and 1.5 mol of potassium citrate and mixing them to prepare a tempered glass composition.

[0125] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 1.

[0126] Comparative Example 14

[0127] This comparative example provides a strengthened glass composition, and the strengthened glass composition is the same as that of comparative example 13.

[0128] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 2.

[0129] Comparative Example 15

[0130] This comparative example provides a strengthened glass composition, and the strengthened glass composition is the same as that of comparative example 13.

[0131] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 3.

[0132] Comparative Example 16

[0133] This comparative example provides a strengthened glass composition, and the strengthened glass composition is the same as that of comparative example 13.

[0134] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those of Example 4.

[0135] Comparative Example 17

[0136] This comparative example provides a strengthened glass composition, comprising: taking 1 mol of potassium sulfite and 2 mol of potassium ethoxide and mixing them to prepare a strengthened glass composition.

[0137] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 1.

[0138] Comparative Example 18

[0139] This comparative example provides a strengthened glass composition, comprising: taking 0.6 mol potassium sulfite and 2.4 mol potassium citrate and mixing them to prepare a strengthened glass composition.

[0140] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 1.

[0141] Comparative Example 19

[0142] This comparative example provides a strengthened glass composition, comprising: taking 2.4 mol potassium sulfite and 0.6 mol potassium citrate and mixing them to prepare a strengthened glass composition.

[0143] This comparative example also provides a chemical strengthening process for glass, and the process parameters and methods are the same as those in Example 1.

[0144] Experimental Example 1

[0145] In this experimental example, the chemically strengthened glasses obtained in Examples 1-19 and Comparative Examples 1-19 were subjected to surface stress tests or glass warpage tests.

[0146] Surface stress test method: Test according to GB / T18144-2008 glass stress test method.

[0147] Glass warpage test method: Place the chemically strengthened glass at room temperature for 4 hours, and then use a feeler gauge to measure the arc height h and chord length L of the chemically strengthened glass; the glass warpage is expressed as the percentage of the arc height to the chord length. The schematic diagram of the arc height h and the chord length L is shown in Figure 1 .

[0148] The test results of surface stress are shown in Table 1 below. Compared with Comparative Examples 9-18, the strength of the chemically strengthened glasses obtained in Examples 1-19 is higher, as shown by the surface stress of the chemically strengthened glasses being between 83 and 140 MPa. Among them, compared with Examples 5-12, Examples 1-4 use potassium sulfite: potassium hydroxide: potassium sorbate = 0.5:0.5:2 as the strengthened glass composition, which further improves the surface stress of the chemically strengthened glass, and Example 1 is the best.

[0149] Table 1 Test results

[0150]

[0151]

[0152] The warpage test results are shown in Table 2 below. Compared with Comparative Examples 1-8 and 17-19, the warpage of the chemically strengthened glass obtained in Examples 1-19 is between 0.11% and 0.28%, and the warpage phenomenon is greatly improved.

[0153] Table 2 Warpage measurement results

[0154]

[0155] Experimental Example 2

[0156] In this experimental example, the thickness of the compressive stress layer of the chemically strengthened glass obtained in Examples 1-18 and Comparative Examples 1-16 was tested according to the testing method for the thickness of the compressive stress layer in Chemically Tempered Glass (JC / T 977-2005).

[0157] The test results are shown in Table 3. The compressive stress layer thickness of the chemically strengthened glass prepared in Examples 1-18 is relatively small, and meets the use requirements of the intermediate layer glass of insulating glass, that is, meets the Class A requirements in the standard "Chemically Tempered Glass" (JC / T977-2005), 12μm<compressive stress layer thickness≤25μm, which can ensure the safety of the use of the intermediate layer glass, and ensure the surface structure and safety of the intermediate layer glass.

[0158] Table 3 Measurement results

[0159]

[0160]

[0161] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A tempered glass composition, characterized in that: It comprises an inorganic potassium salt and an organic potassium salt, wherein the molar ratio of the inorganic potassium salt to the organic potassium salt is 1-3:1-2; The inorganic potassium salt is selected from at least one of potassium nitrate, potassium chloride, potassium sulfate, potassium sulfite, potassium phosphate, dipotassium hydrogen phosphate, potassium dihydrogen phosphate, and potassium hydroxide; The organic potassium salt is selected from at least one of potassium benzoate, potassium citrate and potassium sorbate.

2. The tempered glass composition according to claim 1, wherein The strengthened glass composition comprises potassium sulfite, potassium hydroxide and potassium sorbate; preferably, the molar ratio of potassium sulfite, potassium hydroxide and potassium sorbate is 0.5-1:0.5-1:

2.

3. A method for preparing a tempered glass composition according to claim 1 or 2, characterized in that: The preparation method comprises the steps of taking an organic potassium salt and an inorganic potassium salt according to the above molar ratio, mixing them, and obtaining the product.

4. Use of the tempered glass composition obtained according to claim 1 or 2 or the method for preparing the tempered glass composition according to claim 3 in glass strengthening.

5. A chemical strengthening process for glass, characterized in that: Strengthening glass by solvent method, molten salt method or slurry method; The solvent method comprises mixing the tempered glass composition according to claim 1 or 2 or the tempered glass composition prepared by the method for preparing the tempered glass composition according to claim 3 with solvent 1 to obtain a mixture, and then coating the mixture on a glass surface and drying to obtain the tempered glass; The molten salt method comprises heating the tempered glass composition according to claim 1 or 2 or the tempered glass composition prepared by the method for preparing the tempered glass composition according to claim 3 to obtain molten salt, coating the molten salt on the surface of the glass, and drying to obtain the tempered glass; The slurry method comprises mixing the tempered glass composition according to claim 1 or 2 or the tempered glass composition prepared by the method for preparing the tempered glass composition according to claim 3 with a solvent 2 and a binder to prepare a mixture, applying the mixture on a glass surface, and drying to obtain the tempered glass.

6. The chemical strengthening process for glass according to claim 5, characterized in that: In the solvent method, the solvent 1 is selected from water and / or ethanol; and / or the ratio of the volume of the solvent 1 to the mole of the tempered glass composition is 100-700 mL:2-4 mol; and / or the drying step comprises first drying at a temperature of 80-170° C. for 5-25 min, then heating the temperature to 220-300° C. at a heating rate of 10-30° C. / min, and keeping the temperature at 220-300° C. for 20-60 min.

7. The chemical strengthening process for glass according to claim 5, characterized in that: In the slurry method, the binder is selected from clay and / or diatomaceous earth; and / or the solvent 2 is selected from water and / or ethanol; and / or the ratio of the mole of the tempered glass composition, the volume of the solvent 2 and the mass of the binder is 2-4 mol:100-700 mL:50-200 g; and / or the drying step comprises first drying at a temperature of 50-100° C. for 20-50 min, then heating the temperature to 150-250° C. at a heating rate of 8-25° C. / min, and keeping the temperature at 150-250° C. for 60-120 min.

8. The chemical strengthening process for glass according to any one of claims 5 to 7, characterized in that: In the molten salt method, the heating temperature is 240-430°C; and / or the drying step includes first drying at a temperature of 80-170°C for 5-20 minutes, then heating the temperature to 220-300°C at a heating rate of 5-20°C / min, and keeping the temperature at 220-300°C for 20-60 minutes.

9. The chemical strengthening process for glass according to any one of claims 5 to 8, characterized in that: The coating method in the solvent method, molten salt method or slurry method is selected from at least one of brushing, printing and spraying; and / or, the solvent method, molten salt method or slurry method further includes cooling and cleaning steps after drying.

Citation Information

Patent Citations

  • Safety strengthening agent in touch-control glass tempering process

    CN104710105A

  • Processing method for 3D glass, glass cover plate and mobile terminal

    CN109592906A

  • Composition for glass strengthening, preparation method thereof and glass strengthening method

    CN113480196A

  • Glass tempering treatment process

    CN114835387A

  • Tempered glass composition as well as preparation method and application thereof

    CN117658479A