High-permeability quartz yarn and preparation method thereof
By using quartz yarn wetting agent with specific solid content and polar components to surface treatment, the problem of difficult to explore the influence of chemical composition in the study of permeability of glass fiber preforms is solved, and high permeability is achieved The preparation of quartz yarn composite materials provides a rapid penetration performance research method and a basis for the development of functional wetting agents.
Patent Information
- Application Number
- CN202411128581.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
In the study of the permeability properties of glass fiber preforms, the influence of chemical composition on the surface of glass fiber on the flow and permeability of fiber bundles and related experimental methods are less studied, and the sample preparation is complicated and the testing device is expensive, resulting in fiber bundles. Intraflow and permeability experiments are difficult to perform.
The quartz yarn composite with high permeability is prepared by infiltration and drying steps using quartz yarn wetting agents with specific solid content and polar component content. Material.
Effectively regulating the permeability of quartz yarns provides a quick way to study the permeability of quartz fiber bundles in the industrial field, providing a basis for the development of functional wetting agents, and improving the permeability of yarns.
Smart Images

Figure CN118993577A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material preparation, in particular to a high-permeability quartz yarn and a preparation method thereof. Background Art
[0002] Quartz yarn is a high-performance glass fiber material made from high-purity quartz or natural crystal with a SiO2 content of more than 99.9%. With excellent mechanical, high temperature resistance, electrical insulation, ablation resistance and good chemical stability, glass fiber reinforced composite materials (GFRC) are widely used in optical fiber, electronics, aerospace, rail transportation, machinery manufacturing and other industrial fields.
[0003] With the development of new liquid molding (LCM) technology, GFRC has significant technical advantages in the manufacture of products with complex shapes and highly concentrated loads, and its application prospects are broader. However, the flow and permeability of resin solution in glass fiber preforms are key factors in reducing processing cycles and improving product comprehensive performance in LCM technology, and have always been a research hotspot in the professional field.
[0004] In terms of the permeability of glass fiber preforms, researchers have done a lot of fruitful research. The first is to construct a multi-dimensional theoretical prediction, based on Darcy's law and Kozeny-Carman formula, comprehensively consider factors such as resin volume flow rate, fiber volume and porosity, and use finite element analysis and computer numerical simulation methods to form a permeability prediction model; the second is the experiment and characterization of permeability, usually using one-dimensional unidirectional method and two-dimensional bidirectional (radial) method to test the actual permeability of different types of preforms, including flat fabrics, non-woven fiber mats, three-dimensional thick fabrics and anisotropic fabrics. More research is carried out around the influencing factors and laws of fiber preform permeability, such as the influence of different material mixed structures, fiber layup, fiber compression, fiber flow channels and flow direction on permeability, and the influence of materials such as carbon nanotubes sprayed on the surface of glass fiber fabrics on the permeability of glass fiber fabrics.
[0005] In recent years, scientific researchers have paid more and more attention to and studied the permeability of fiber bundles. Verpoest et al. proposed that the permeability is restricted by factors such as the pores between fiber bundles, the wicking effect of fibers within the fiber bundles, and the capillary pressure. Weitzenbock considered the large voids between fiber bundles and the micropores between single fibers within the fiber bundles, proposed the competitiveness of resin permeability between large voids and micropores, and established a theoretical model for fiber bundle permeability. Wei Yajun ignored the influencing factors such as internal chemical reactions and surface tension, fully considered the differences in the spacing between fiber bundles and the spacing between fibers within the fiber bundles, established a dual-scale geometric model, and improved the accuracy of permeability prediction results. Patel used a dynamic contact angle tester to characterize the permeability of fiber bundles and its correlation with porosity based on the wicking experimental results of fiber bundles. Amin constructed a wicking performance model for fibers in ordered and disordered directions, and developed a new experimental method to verify its rationality. Willenbacher built a new test device to characterize the out-of-plane capillary pressure of fibers with different volume contents.
[0006] In summary, the permeability of the preform is the result of the coordinated flow of the resin between and within the fiber bundles. The permeability of the resin within the fiber bundle has a great influence on the fluidity of the preform. The factors that affect the flow resistance within the fiber bundle, such as the volume fraction of glass fibers, fiber gaps, fiber orientation, and fiber capillary pressure, have been relatively well studied. However, there are few studies on the effects of the chemical composition of the glass fiber surface on the flow and permeability of the fiber bundle, and there are also few studies on experimental methods for flow and permeability within the fiber bundle. In addition, there are problems such as complex sample preparation and expensive test equipment / instruments. Summary of the invention
[0007] The purpose of the present invention is to provide a high-permeability quartz yarn and a preparation method thereof to solve the problems existing in the above-mentioned prior art.
[0008] To achieve the above object, the present invention provides the following solutions:
[0009] The present invention provides a quartz yarn impregnating agent, the raw material components of the impregnating agent include a coupling agent, a film-forming agent and a lubricant;
[0010] The solid content of the quartz yarn impregnation agent is 6.10-6.50wt%, and the polar component content is 59.02-61.54wt%;
[0011] The solid content is the mass proportion of the coupling agent, film-forming agent and lubricant in the quartz yarn impregnating agent;
[0012] The polar components are coupling agents and film formers.
[0013] Furthermore, the coupling agent includes a silane coupling agent.
[0014] More specifically, the coupling agent can be a silane coupling agent with moderate water solubility and hydrolysis activity, used alone or in combination, including coupling agents containing amino groups and epoxy groups, such as γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γaminopropyltrimethoxysilane, γ-glycidyl ether propyltrimethoxysilane, etc.
[0015] Furthermore, the film-forming agent includes epoxy resin and / or polyester resin.
[0016] More specifically, the film-forming agent may be a water-soluble polymer material with a group that is prone to nucleophilic and electrophilic reactions, including an alcohol-based epoxy resin solution (relative molecular weight of 200-1000, such as glycerol epoxy resin) and a maleic anhydride-based polyester resin solution (relative molecular weight of 1000-5000, such as polyvinyl alcohol polyester resin, diethylene glycol polyester resin, diethylene glycol polyester resin, etc.). Usually, the epoxy resin solution and the polyester resin solution are used alone and / or in combination.
[0017] Furthermore, the lubricant includes a cationic lubricant and / or a non-ionic lubricant.
[0018] More specifically, the lubricant may be a cationic lubricant (relative molecular weight 200-500, such as C 18 Fatty amide, C 16 Emulsions containing either fatty amides) or non-ionic lubricants (relative molecular weight 200-500, such as polyethylene glycol, stearyl alcohol, and palmityl alcohol) alone or in combination.
[0019] The present invention also provides a method for preparing a quartz yarn composite material, comprising the following steps: using the quartz yarn impregnating agent to perform surface treatment on the quartz yarn. The surface treatment is impregnation.
[0020] Furthermore, the surface treatment further includes a drying step; the drying temperature is 105°C.
[0021] Furthermore, the quartz yarn has a linear density of 190 tex, a twist of 70 twists, and a single yarn diameter of 7.5±1.0 μm.
[0022] The present invention further provides a quartz yarn composite material prepared by the above preparation method.
[0023] The present invention discloses the following technical effects:
[0024] The present invention uses a wetting agent with a specific solid content and polar component content to perform surface treatment on the quartz yarn, thereby ensuring the excellent permeability of the quartz yarn. The present invention regulates the permeability of the quartz yarn from a chemical perspective, provides a quick method for studying the permeability of quartz fiber bundles in the industrial field, and provides a basis for developing functional wetting agents. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 are the pH value (a) and viscosity (b) of different wetting agents;
[0027] Figure 2 Horizontal (a) and vertical (b) penetration curves of quartz yarn after RFS infiltration and horizontal (c) and vertical (d) 3-min penetration length images;
[0028] Figure 3 Surface energy (a), dynamic contact angle (b) and image (cf) of quartz yarn after wetting;
[0029] Figure 4 The morphological images of quartz yarns DS (a, e, f), YS (b, g, h), YS90 (c, i, j), and YS95 (d, k, l) after infiltration;
[0030] Figure 5 The adhesive rate of the quartz yarn after infiltration (a) and the appearance of the YS yarn after infiltration and burning (b);
[0031] Figure 6 Diameter and distribution of quartz fiber after infiltration; (a) is DS, (b) is YS, (c) is YS90, and (d) is YS95;
[0032] Figure 7 Diameter and distribution of quartz yarn after infiltration under constant tension; (a) DS, (b) YS, (c) YS90, (d) YS95;
[0033] Figure 8 The infrared spectrum (a) and magnified spectrum (b) of quartz yarn after infiltration;
[0034] Fig. 9 EDS element analysis spectra of quartz yarn after infiltration; (a) is DS, (b) is YS, (c) is YS90, and (d) is YS95;
[0035] Fig.10 The possible reaction mechanisms of the wetting agent components are: (a) reaction of normal coupling agent content; (b) reaction between coupling agent molecules; (c) reaction between coupling agent and film-forming agent; (d) reaction of excessive coupling agent content. DETAILED DESCRIPTION
[0036] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0037] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0038] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0039] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.
[0040] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0041] Aiming at the problem that the permeability of fiber preforms prepared from different quartz fiber bundles (yarns) is significantly different, a new sizing agent is developed to improve the permeability of yarns, and the influence of polar component content (COP) and solid content (COS) such as coupling agent and film-forming agent on the permeability, wetting and bundling of yarns and the influence of the content and mechanism of action, and the performance of commercial quartz yarns with high permeability are compared. The results show that when COP and COS are the lowest (59.02 and 6.10wt%), the permeability of quartz yarn is the highest, and the vertical 3min permeation length (LV3) and the horizontal 3min permeation length (LH3) are 7.5 and 17.9mm respectively; when COP and COS are the highest (61.54 and 6.50wt%), the permeability is the lowest (LV3 and LH3 are 6.9 and 17.6mm respectively); the permeability of the prepared yarns is better than that of commercial yarns (LV3 and LH3 are 6.4 and 17.1mm respectively). When COS is the highest, the number of large flakes on the surface of the yarn (SEM image) and the adhesive rate (0.92wt%) are relatively high, and the bundling is large (the average diameter of the yarn is 0.71mm). The bonding effect of the large flakes may reduce the gap between the yarn fibers. When COP is the highest, the surface energy of the yarn (43.51mN / m), the infrared absorption peaks of O-H and C-O (3443 and 1115cm respectively) -1 ) strength and O / Si atomic ratio (1.73:1.00) are relatively low, which may be due to the condensation reaction between too many coupling agent molecules or between coupling agent and film-forming agent molecules, resulting in a decrease in polar groups such as -OH ( Fig.10 b, c) formation.
[0042] The present invention proposes the mechanism of action of the wetting agent components, further explains that COS and COP may be the key factors affecting the fluidity and permeability of the resin between fibers, supplements the research theory of the permeability of fiber bundles from a chemical perspective, provides a quick characterization method for studying the permeability of fiber bundles in the industrial field, and provides experimental data and reference basis for the development of functional wetting agents.
[0043] The present invention is further described in detail below:
[0044] Example 1
[0045] 1. Materials and Reagents
[0046] Homemade XS-type quartz yarn (linear density 190 tex, twist 70 twists, single filament diameter 7.5 ± 1.0 μm);
[0047] A commercially available impregnated quartz yarn product with excellent permeability is used as a benchmark product for the permeability of the present invention, and is subsequently labeled as DS-type quartz yarn. It has a linear density of 190tex, a twist of 70 twists, and a single filament diameter of 7.5±1.0μm. The product is treated with impregnation and has excellent permeability: the penetration lengths of the yarn in the vertical direction of 60, 120, and 180s are 4.6, 5.7, and 6.4cm, respectively; the penetration lengths in the horizontal direction of 60, 120, and 180s are 13.9, 16.3, and 17.1cm, respectively.
[0048] Precondensed phenolic resin solution (PRF, 50 wt %, viscosity 2.18 mPa·s), Anhui Huaye Special Materials Co., Ltd.;
[0049] Sodium hydroxide (NaOH, AR), formaldehyde (37wt%), Sinopharm Chemical Reagent Co., Ltd.; ethylene glycol (AR), glacial acetic acid (AR), Shanghai MacLean Biochemical Technology Co., Ltd.; silane coupling agent (JH-A10), film-forming agent (CM-170), lubricant (RH-307); deionized water.
[0050] 2. Sample Preparation
[0051] a. Preparation of phenolic resin solution (RFS)
[0052] 2.25 g of NaOH was added to 80 g of deionized water, and the mixture was stirred on a magnetic stirrer at 300 rpm for 5 min. Then, 10.0 g of PRF solution was added and stirred for 10 min. 4.0 g of formaldehyde was added, and the reaction was continued by stirring for 4 h to obtain a phenolic resin solution (RFS).
[0053] b. Preparation of functional quartz yarn (YS series)
[0054] Deionized water and glacial acetic acid were added to the coupling agent (silane coupling agent), and magnetic stirring was performed for 1 hour. A film-forming agent, a lubricant and deionized water were added and stirred for 5 minutes to prepare wetting agents with different solid contents. After the formula was enlarged, it was used to process YS type high permeability quartz yarn. According to the different wetting agent formulas (Table 1), they were named YS, YS90 and YS95 yarns respectively.
[0055] Specifically: After the XS type quartz yarn is surface treated with different impregnants, it is dried at 105° C. for 2 hours and placed in a dryer for standby use.
[0056] Table 1 Main component proportion and solid content (COS) of sizing agent corresponding to different functional yarns
[0057] Main Ingredients YS Yarn Sizing YS90 Yarn Sizing Agent YS95 Yarn Sizing Agent <![CDATA[Coupling agent ① , wt%]]> 15.38 14.75 15.08 <![CDATA[Film-forming agent ① , wt%]]> 46.16 44.27 45.24 <![CDATA[Lubricant ② , wt%]]> 38.46 40.98 39.68 COS, wt% 6.50 6.10 6.30
[0058] Note: ①-COP (polar component), ②-Non-COP (non-polar component). COS is the percentage of coupling agent, film former and lubricant in the wetting agent.
[0059] pH value and dynamic viscosity of the wetting agent:
[0060] The viscosity of the infiltrant was measured using the NDJ-5S rotary viscometer from Shanghai Changji Geological Instrument Co., Ltd., with rotor No. 0 selected. The pH value of the infiltrant was tested using a PHS-3C pH meter. The sample temperature was 25°C.
[0061] pH value and dynamic viscosity of the sizing agent for YS, YS90 and YS95 yarns are shown in Figure 1 The pH of the three wetting agents is similar ( Figure 1 a); but the order of viscosity from large to small is YS>YS95>YS90( Figure 1 b), indicating that the intermolecular forces of the YS-type wetting agent are the strongest, which may be related to the higher COS of the wetting agent and the higher COP content of coupling agents and film-forming agents (Table 1).
[0062] Material performance characterization:
[0063] The properties of the impregnated quartz yarn are characterized as follows:
[0064] 1. Quartz yarn penetration performance
[0065] Two methods were used to characterize the penetration performance of RFS in quartz yarn:
[0066] (1) Horizontal penetration length
[0067] Take a 30cm quartz yarn, straighten it and fix both ends on a horizontal glass plate (the glass plate is fixed with a ruler along the yarn direction), take 20μL RFS and drop it in the center of the yarn, and use video to record the penetration length of RFS in the yarn. When multiple yarns are tested at the same time, they need to be fixed on the glass plate in parallel, with a yarn spacing of ≥4cm. Draw the penetration curve within 3min (collect penetration length data every 5s).
[0068] (2) Vertical penetration length
[0069] Take a 21cm quartz yarn, clamp both ends with sample clamps (the length of the yarn clamped by the two clamps is 0.5cm, and the yarn is evenly stressed between the two clamps), fix the head end on a horizontal rod, and let the tail end hang vertically under a constant tension hammer. When multiple yarns are tested at the same time, the yarn interval is ≥3cm. Fix a scale ruler along the yarn direction. Add 50g RFS quantitatively to a glass dish and place it on a lifting platform. Adjust the position of the glass dish so that the tail end of the yarn is aligned with the center of the glass dish. Slowly raise the lifting platform until RFS submerges the tail end sample clamp by 0.5cm. Use video to record the penetration length of RFS in the yarn. Draw a penetration curve within 3 minutes (penetration length data is collected every 5 seconds).
[0070] The horizontal penetration curves and 3-min penetration length images of RFS in DS and YS series quartz yarns are shown in Figure 2 a and Figure 2 c. It can be seen that the horizontal penetration lengths of DS, YS, YS90 and YS95 yarns at 60, 120 and 180 s are (13.9, 14.3, 15.1, 14.7), (16.3, 16.8, 17.1, 16.9) and (17.1, 17.6, 17.9, 17.7) cm, respectively. Figure 2 a), the order of horizontal penetration length after stabilization (≥60s) is YS90>YS95>YS>DS type. The penetration performance of YS90 and YS95 types is similar, but the comprehensive performance of YS90 type is the best. The analysis shows that the permeability difference between DS and YS series may be related to the yarn components, preparation process and sizing agent composition, but under the same conditions of yarn components and preparation process, the permeability difference between YS, YS90 and YS95 types mainly depends on the sizing agent composition.
[0071] The essence of yarn permeability is the flow performance of the resin, that is, the larger the gap between the fibers inside the yarn or the smaller the interaction force between the fibers, the smaller the resin flow resistance and the better the yarn permeability. Further analysis shows that due to the excessive COP and COS of coupling agents in the YS impregnation film, more macromolecular sheets may be formed through physical accumulation or chemical reaction, which enhances the bonding and interaction between the fibers, resulting in a decrease in the gap between the fibers, an increase in the resin flow resistance, and a decrease in the permeability. On the contrary, the YS90 impregnation agent has the largest content of non-polar components such as lubricants and the smallest COS, so the intermolecular force and bonding effect of the impregnation film on the fiber surface are relatively small, the resin flow resistance is small, and the yarn permeability is the best. Therefore, the high COP content and large COS of the impregnation agent may be the key factors in reducing the permeability of the yarn.
[0072] The vertical penetration curves and 3-min penetration length images of RFS in DS and YS series quartz yarns are shown in Figure 2 b and Figure 2d. It can be seen that the horizontal penetration lengths of DS, YS, YS90 and YS95 yarns at 60, 120 and 180 s are (4.6, 4.8, 5.4, 5.3), (5.7, 6.2, 6.7, 6.7) and (6.4, 6.9, 7.5, 7.3) cm, respectively. Figure 2 b), the vertical permeability order is YS90>YS95>YS>DS, the permeability of YS90 and YS95 is similar and significantly better than that of YS and DS, and YS90 has the best comprehensive performance. The permeability law of quartz yarn measured by the vertical method is consistent with that of the horizontal method.
[0073] Depend on Figure 2 It can also be seen that the permeation curve of the quartz yarn in the horizontal direction gradually flattens, and the permeation rate shows a gradually decreasing trend. Analysis shows that since RFS is quantitatively poured, as the permeation distance increases, the concentration of RFS at the permeation site becomes lower and lower, and the permeation rate becomes smaller and smaller. The concentration gradient may be an important factor affecting the permeation rate trend.
[0074] Permeation curve and permeation rate of quartz yarn in vertical direction ( Figure 2 b) The regularity is consistent with the horizontal test results, but the penetration rate and penetration distance are significantly reduced. Analysis shows that during the upward penetration along the yarn, the reverse effect of its own gravity weakens the concentration and flow rate of RFS at the diffusion site. The magnitude and direction of the force are important factors affecting the resin penetration performance.
[0075] 2. Surface energy and dynamic contact angle of quartz yarn
[0076] The surface energy and dynamic contact angle of the yarn were tested using a DCAT11 surface tension meter produced by German dataphysics company.
[0077] After the dynamic contact angle of the yarn was measured using deionized water and ethylene glycol, OWRK was selected to calculate the surface energy of the yarn. The dynamic contact angle of the yarn was tested using RFS, the sample shape was selected as Circle, the diameter parameter was 0.7mm, the liquid level detection motor speed was 0.5mm / s, the advancing angle and receding angle test motor speed was 0.2mm / s, the liquid level detection accuracy was 1mg, the yarn immersion depth was 3mm, the experimental repetition number was 1, and the advancing angle and receding angle dwell interval was 0s. Each yarn was tested in 3 groups (3 samples / group), and the sum of the median values of each group was taken to calculate its average value.
[0078] Surface energy, dynamic contact angle and image of quartz yarn are shown in Figure 3 The surface energies of DS, YS, YS90 and YS95 yarns are 48.28, 43.51, 42.81 and 55.58 mN / m, respectively. Figure 3a), and the dynamic contact angles are 26.24, 34.03, 34.56 and 24.45 mN / m ( Figure 3 b), the surface energy (surface tension) of the yarn is positively correlated with its wettability, that is, the higher the surface energy of the yarn, the better the wetting performance of RFS on the yarn (the smaller the dynamic contact angle). However, under the premise of good wetting (the dynamic contact angle of the yarn is much less than 90°), the wettability of the YS series yarn (YS95>YS>YS90, Figure 3 b) and permeability (YS90>YS95>YS, Figure 2 ) did not show a positive correlation, YS had better wettability but the lowest permeability, and YS90 had the lowest wettability but the best permeability.
[0079] Since surface tension is mainly the result of intermolecular interactions (hydrogen bonding force, induction force, orientation force and dispersion force), the more polar molecules there are, the stronger the induction force and orientation force are, and the greater the surface tension is. However, the COP content in the YS sizing agent is the highest, but the surface tension is relatively small ( Figure 3 a). It is believed that during the coating and drying process of the sizing agent, the excessive coupling agent in the YS sizing agent (beyond the monomolecular coating layer) may undergo chemical cross-linking reactions with more film-forming agent molecules to form macromolecular aggregates, reduce the content of film-forming agent and its polar groups on the surface of the fiber sizing film, and relatively increase the content of non-polar lubricant, resulting in a decrease in the surface tension of the sizing film ( Fig.10 d). That is, the content of coupling agent and film former in the sizing agent and their reactivity may have an important influence on the wetting properties of the yarn.
[0080] 3. Surface morphology, element content, fiber fineness and adhesive rate of quartz yarn
[0081] The quartz yarn was gold-sprayed, and its surface morphology was observed using a Hitachi S-4800 scanning electron microscope, and the elements and content of the yarn were tested using an X-ray energy dispersive spectrometer (EDS S-4800). Nano measure software was used to characterize the fiber fineness and distribution.
[0082] The quartz yarn was placed in a muffle furnace and burned at 625℃ for 2h, weighed and the adhesive rate was calculated according to formula (1):
[0083] X = 100% × (m0-m1) / m1 (1)
[0084] Where: X is the adhesive rate, %; m0 is the mass of the quartz yarn before burning, g; m1 is the mass of the quartz yarn after burning, g.
[0085] Figure 4The appearance of quartz yarn at different magnifications. It can be seen that the surface of DS-type quartz yarn (a, e, f) is smooth, the wetting agent is evenly distributed (the coating thickness is at the nanometer level), and there are a small number of small dispersed particles on the fiber surface (as shown by the arrow in Figure f); the surface of YS-type quartz yarn (b, g, h) is smooth, but the wetting agent is not evenly distributed, and there are more dispersed layers on the fiber surface (as shown by the arrow in Figure h); compared with YS type, the size and number of dispersed particles of the wetting agent on the fiber surface of YS90 (c, i, j) and YS95 (d, k, l) quartz yarn are significantly reduced, and YS90 type has the least. Analysis shows that under production and processing conditions, the excessive coupling agent in the YS-type wetting agent will chemically cross-link with the film-forming agent to form a film covering and bonding on the fiber surface, which seriously affects the uniformity of the gaps between the fibers inside the yarn, and then increases the flow resistance of the resin and reduces the permeability of the yarn.
[0086] Figure 5 It is the adhesive rate of quartz yarn and the appearance of YS yarn after burning. It can be seen that the surface of quartz yarn after burning is clean, indicating that the impregnation agent is well removed under the experimental conditions ( Figure 5 b); The rubber content of DS, YS, YS90 and YS95 yarns are 0.83, 0.92, 0.85 and 0.93% respectively ( Figure 5 a). The rubber content of YS and YS95 yarns is slightly higher, which further confirms the above SEM observation results. However, the rubber content of YS and YS95 yarns is relatively consistent, and the permeability is quite different, indicating that within a certain range, the effect of the single factor rubber content on the permeability is not obvious.
[0087] Figure 6 Figure 2 shows the fiber diameter and distribution of quartz yarn. It can be seen that the average fiber diameter of DS quartz yarn is smaller (7.39 μm). The fiber diameter and distribution of YS series quartz yarn are similar (8.67, 8.62 and 8.61 μm), indicating that the process of YS yarn preparation is stable and the fiber fineness is uniform.
[0088] 4. Bunching performance of quartz yarn
[0089] Fix a straight tube with a clip and a ruler (≥20cm) on an iron stand, clamp a quartz yarn with a length of 21cm at 0.5cm from the end, and then clamp the end at 0.5cm with a clip, paying attention to maintaining the original twist and uniform stress state of the yarn (all clips are of equal size and weight). When multiple yarns are tested at the same time, the yarn spacing is equal and ≥2cm. Use images to record the stable state of the yarn, and use nano measure software to accurately measure its diameter to characterize the bundling performance of the yarn.
[0090] Figure 7The following is the bundling property (characterized by yarn diameter, the smaller the diameter, the higher the bundling property) and yarn diameter distribution diagram of quartz yarn under constant tension conditions. It can be seen that there is no positive correspondence between the average diameters of DS, YS, YS90 and YS95 yarns (0.83, 0.71, 0.81 and 0.81 mm, respectively) and the fiber diameters (7.39, 8.67, 8.62 and 8.61 μm, respectively). The fiber bonding of YS quartz yarn is tight and the bundling property is high, while the fiber bonding of YS90 and YS95 yarns is tight and the bundling property is relatively low. The bundling property of DS and YS90 / YS95 yarns is similar and the permeability is quite different. The bundling property of DS and YS yarns is quite different and the permeability is similar, indicating that the influence of the single factor bundling property on the permeability performance is not obvious.
[0091] Compared with YS90 / YS95, YS yarn has a small diameter, high bundling and low permeability. The analysis shows that the film blocks and large particles formed by cross-linking of excessive coupling agents and film-forming agents on the surface of YS yarns tightly connect the fibers based on chemical bonding and physical adsorption. The gaps between the fibers are too small or cannot form complete capillaries, which increases the movement resistance of the resin in the fiber gaps and reduces the permeability of the yarn. At the same time, the polar groups in the film-forming agent may lead to greater intermolecular forces on the fiber surface and also form greater flow resistance to the resin. It shows that the content of the wetting agent COS and COP has a significant effect on the bundling of the yarn, which in turn affects the permeability.
[0092] 5. Changes in Surface Groups of Quartz Yarn
[0093] The yarn was cut into pieces (about 5 mm) and evenly mixed with KBr, ground for 5 min, and pressed into thin sheets. The changes in the yarn surface groups were analyzed using the IRPrestige-21 Fourier transform infrared spectrometer (FTIR) of Shimadzu Company, Japan, with a wave number range of 4000-500 cm –1 , resolution 4cm –1 .
[0094] Figure 8 and 9 This is the infrared absorption and elemental analysis spectrum of quartz yarn. Figure 8 It can be seen that DS, YS, YS90 and YS95 yarns all have four stretching vibration characteristic absorption peaks, namely O—H (3443cm -1 )、C—O(1115cm -1 ) and Si—O (965 and 798 cm -1 , respectively asymmetric and symmetric stretching vibrations (a small amount of C-N peak and C-O peak overlap in the impregnant). -1At the absorption peak, the absorption peak intensity of YS yarn is lower than that of YS90 and YS95 yarns, indicating that the content of hydroxyl and ether oxygen bonds in YS yarn is significantly less. This is inconsistent with the high COP content such as hydroxyl in the YS90 sizing agent formula. Analysis shows that at the product processing temperature, an appropriate amount of coupling agent may undergo condensation and addition reactions with glass fiber and film-forming agent, losing hydroxyl groups in the form of H2O molecules, and the lubricant is dispersed between the film-forming agent molecules on the surface of the sizing film ( Fig.10 a). The more coupling agent components there are, the more reactions there are between coupling agent molecules or between coupling agent and film-forming agent molecules ( Fig.10 b, c) The more water molecules are lost, the more the polar O-H and C-O absorption peaks of the YS yarn surface wetting film are reduced ( Fig.10 d).
[0095] The atomic ratios of O / Si / C (the peak position of N atoms overlaps with that of oxygen atoms) of DS, YS, YS90, and YS95 are 1.97 / 1.00 / 0.41, 1.73 / 1.00 / 0.38, 1.95 / 1.00 / 0.72, and 1.68 / 1.00 / 0.69, respectively. Fig. 9 ), the O / Si atomic ratios of YS and YS95 are close and significantly lower than that of YS90. It may be that the excessive coupling agent in the YS90 wetting agent (exceeding the amount used to form a monolayer) reacts with the film-forming agent to form an addition and condensation reaction, resulting in a decrease in the number of oxygen atoms ( Fig.10 d). Further analysis shows that when the quartz fiber components, fineness and preparation conditions are exactly the same, the content of silanol on the fiber surface is similar, and the theoretical amount of coupling agent to react with it is the same, and the total number of oxygen atoms eliminated is the same (equivalent to each coupling agent molecule eliminating 2 water molecules, Fig.10 a); Excessive coupling agent molecules can react with other molecules to eliminate 3 water molecules ( Fig.10 b, c). Therefore, when the coupling agent content is too high, the O / Si atom ratio is low.
[0096] In summary: regulating the solid content of the sizing agent and the mass ratio of polar components such as coupling agents and film-forming agents to non-polar components such as lubricants can effectively regulate the permeability of the fibers in the quartz yarn bundle; the content of polar components such as coupling agents and film-forming agents and their reaction results are key factors affecting the surface tension of quartz fibers and the interaction between fibers; if the solid content of the sizing agent is too high, more macromolecular sheets may be formed through physical accumulation or chemical reaction, thereby increasing the adhesion between fibers. Both of them are based on affecting the flow resistance of the resin between fibers and further affecting the permeability; a single factor among the surface energy, wettability, bundling, and adhesive attachment rate of the yarn has no obvious corresponding relationship with the permeability of the fibers in the yarn bundle.
[0097] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A quartz yarn sizing agent, characterized in that: The raw materials include coupling agents, film formers and lubricants; The solid content of the quartz yarn impregnation agent is 6.10-6.50wt%, and the polar component content is 59.02-61.54wt%; The solid content is the mass proportion of the coupling agent, film-forming agent and lubricant in the quartz yarn impregnating agent; The polar components are coupling agents and film formers.
2. The quartz yarn sizing agent according to claim 1, characterized in that: The coupling agent includes a silane coupling agent.
3. The quartz yarn sizing agent according to claim 1, characterized in that: The film former includes epoxy resin and / or polyester resin.
4. The quartz yarn sizing agent according to claim 1, characterized in that: The lubricant includes a cationic lubricant and / or a nonionic lubricant.
5. A method for preparing a quartz yarn composite material, characterized in that: The method comprises the following steps: surface treating the quartz yarn using the quartz yarn impregnating agent according to any one of claims 1 to 4.
6. The preparation method according to claim 5, characterized in that: The method further comprises a drying step after the surface treatment; the drying temperature is 105°C.
7. The preparation method according to claim 5, characterized in that: The quartz yarn has a linear density of 190 tex, a twist of 70 twists, and a single yarn diameter of 7.5±1.0 μm.
8. The quartz yarn composite material prepared by the preparation method according to any one of claims 5 to 7.
Citation Information
Patent Citations
Impregnating compound for non-alkali glass fiber direct yarn for epoxy high-pressure pipeline
CN103771732A
Glass fiber direct roving impregnating compound and preparation method and application thereof
CN113213781A
Glass fiber impregnating compound as well as preparation method and application thereof
CN117550816A
Glass fibre coated with a sizing composition containing polyvinyl acetate, ethylene-vinyl acetate copolymer and epoxy resin, used for production of resin-fibre composites by open-mould or closed-mould methods
FR2864072A1