Graphene oxide dispersion liquid, graphene oxide modified cement mortar and preparation method and application of graphene oxide modified cement mortar
Through the graphene oxide dispersion modified by sulfonic acid and tea polyphenols, the problem of reduced fluidity and limited performance improvement in graphene oxide in cement mortar is solved, and the flowability and compressive strength of cement mortar is significantly improved.
Patent Information
- Application Number
- CN202411212413.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Graphene oxide reduces fluidity in cement mortar and has limited effect on improving flexural strength and compressive strength.
Through the coordinated modification of graphene oxide by sulfonic acid groups and tea polyphenols, its dispersion in a high-calcium and high-alkali environment is improved, graphene oxide dispersion liquid is prepared and added to cement mortar, and the flow is improved. Flexibility and compressive strength.
It significantly improves the flowability and compressive strength of cement mortar, improves the dispersion of graphene oxide in cement mortar, and solves the problem of limited performance improvement of traditional graphene oxide in cement mortar.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and particularly relates to a graphene oxide dispersion and a graphene oxide-modified cement mortar, and a preparation method and application thereof. Background Art
[0002] Concrete is considered the most widely used building material worldwide. As the demand for more complex and durable concrete structures increases, higher performance requirements are placed on concrete. However, traditional concrete types often show performance defects such as cracking, reduced durability and low ductility. Introducing nanomaterials to improve concrete microstructure is one of the most effective ways to reduce concrete cracks, pores and defects.
[0003] As a derivative of graphene, graphene oxide has a two-dimensional single atomic layer structure, has ultra-high strength and flexibility, and has a high specific surface area. It is recognized as the most promising candidate for improving concrete performance. However, due to the presence of oxygen-containing functional groups such as carboxyl, it can react with Ca in the cement environment. 2+ The complexation reaction causes graphene oxide to agglomerate and precipitate. At the same time, the addition of graphene oxide will reduce the fluidity of cement mortar. The existence of these problems is not conducive to improving the overall performance of cement mortar. Summary of the invention
[0004] The purpose of the present invention is to address the defects in the prior art that graphene oxide reduces the fluidity of cement mortar and has limited effect on improving the flexural strength and compressive strength of cement mortar, and to provide a graphene oxide dispersion and graphene oxide-modified cement mortar and a preparation method and application thereof.
[0005] In a first aspect, the present invention provides a method for preparing a graphene oxide dispersion, the preparation method comprising: S1. subjecting graphene oxide and a sulfonic acid source compound to a first modification reaction in a first solution to obtain sulfonic acid-modified graphene oxide; S2. subjecting the sulfonic acid-modified graphene oxide obtained in step S1 to a second modification reaction with tea polyphenols in a second solution to obtain a graphene oxide dispersion.
[0006] In some specific embodiments, in step S1, the sulfonic acid source compound is used in the form of a sulfonic acid source compound solution.
[0007] In some specific embodiments, in step S1, the amount of graphene oxide used is 1 to 5 parts by weight, and the amount of the sulfonic acid source compound solution used is 150 to 250 parts by weight.
[0008] In some specific embodiments, in step S2, the amount of tea polyphenols is 0.3-0.7 parts by weight, and the amount of the second solution is 200-400 parts by weight.
[0009] In some specific embodiments, the first modification reaction is a reaction of graphene oxide with a sulfonic acid source compound and a first solution under stirring.
[0010] In some specific embodiments, the stirring time is 20 to 28 hours.
[0011] In some specific embodiments, the second modification reaction is to react the sulfonic acid group-modified graphene oxide obtained in step S1 with tea polyphenols and the second solution under stirring.
[0012] In some specific embodiments, the stirring speed is 4000-6000 rpm, and the stirring time is 1-3 hours.
[0013] In some specific embodiments, the sulfonic acid source compound is selected from at least one of sulfuric acid, sulfurous acid, sodium wood sulfonate, and sodium dodecylbenzene sulfonate.
[0014] In a second aspect, the present invention provides a graphene oxide dispersion prepared by the above method.
[0015] In a third aspect, the present invention provides a graphene oxide-modified cement mortar, wherein the cement mortar contains the above-mentioned graphene oxide dispersion, a water reducer, water, cement and sand, and optional additives and auxiliary materials.
[0016] In some specific embodiments, the content of the graphene oxide dispersion is 15 to 90 parts by weight, the content of the water reducer is 3 to 7 parts by weight, the content of the pure water is 150 to 250 parts by weight, the content of the cement is 300 to 500 parts by weight, the content of the sand is 1000 to 1500 parts by weight, the content of the additive is 0.6 to 2.5 parts by weight, and the content of the auxiliary material is 1.2 to 3.0 parts by weight.
[0017] In a fourth aspect, the present invention further provides the use of the above-mentioned graphene oxide dispersion and / or the above-mentioned graphene oxide-modified cement mortar in the field of building materials.
[0018] The key to the present invention is that the dispersibility of graphene oxide can be improved through the synergistic modification of sulfonic acid groups and tea polyphenols on graphene oxide, especially the dispersibility of graphene oxide in the high-calcium and high-alkalinity environment of cement mortar. When the modified graphene oxide dispersion obtained is added to cement mortar, it can not only improve the fluidity of cement mortar, but also improve the flexural strength and compressive strength of cement mortar. DETAILED DESCRIPTION
[0019] The preparation method of the graphene oxide dispersion provided by the present invention comprises: S1. performing a first modification reaction on graphene oxide and a sulfonic acid source compound in a first solution to obtain sulfonic acid group-modified graphene oxide; S2. performing a second modification reaction on the sulfonic acid group-modified graphene oxide obtained in step S1 and tea polyphenols in a second solution to obtain the graphene oxide dispersion.
[0020] In the present invention, in step S1, the sulfonic acid source compound is a class of compounds that can provide a source of sulfonic acid groups for graphene oxide. The reaction mode can be to add graphene oxide and the sulfonic acid source compound to the first solution at the same time for a first modification reaction, or to first mix the graphene oxide and the first solution evenly and then add the sulfonic acid source compound for the first modification reaction, or to first mix the sulfonic acid source compound with the first solution to obtain a sulfonic acid source compound solution and then add graphene oxide for the first modification reaction. The third reaction mode is preferably adopted, that is, the sulfonic acid source compound is preferably used in the form of a sulfonic acid source compound solution. Among them, the amount of graphene oxide is preferably 1 to 5 parts by weight, such as 1, 2, 3, 4, 5 parts by weight or any value therebetween; the amount of the sulfonic acid source compound solution is preferably 150 to 250 parts by weight, such as 150, 180, 200, 220, 250 parts by weight or any value therebetween. The first solution is preferably water. Controlling the amount of graphene oxide and sulfonic acid source compound solution within the above preferred range is more conducive to improving the fluidity, flexural strength and bending strength of cement mortar when the modified graphene oxide is applied to the cement mortar.
[0021] In the present invention, the sulfonic acid source compound solution can be a solution obtained by mixing a sulfonic acid source compound and a solvent capable of dissolving the sulfonic acid source compound. The present invention does not specifically limit the type of the sulfonic acid source compound, as long as it is a class of compounds containing sulfonic acid groups, and specific examples thereof include but are not limited to: at least one of sulfuric acid, sulfurous acid, sodium wood sulfonate, and sodium dodecylbenzene sulfonate, preferably sulfuric acid. The present invention does not specifically limit the type of the solvent, and preferably water. The present invention does not specifically limit the amount of the sulfonic acid source compound or the concentration of the sulfonic acid source compound in the sulfonic acid source compound solution, that is, when using different types of sulfonic acid source compounds, sulfonic acid source compound solutions with different concentrations can be used, as long as the sulfonic acid groups can be fully grafted onto graphene oxide to obtain sulfonic acid group-modified graphene oxide. When the sulfonic acid source compound used is sulfuric acid, the mass percentage of sulfuric acid in the sulfonic acid source compound solution, i.e., the sulfuric acid solution, is preferably 70-98wt%, such as 70wt%, 75wt%, 80wt%, 85wt%, 90wt%, 95wt%, 98wt% or any value therebetween. When the sulfonic acid source compound used is sodium dodecylbenzene sulfonate, the mass percentage of sodium dodecylbenzene sulfonate in the sulfonic acid source compound solution, i.e., the sodium dodecylbenzene sulfonate solution, is preferably 1-5wt%, such as 1wt%, 2wt%, 3wt%, 4wt%, 5wt% or any value therebetween.
[0022] In the present invention, in step S2, the amount of tea polyphenols is preferably 0.3-0.7 parts by weight, such as 0.3, 0.4, 0.5, 0.6, 0.7 parts by weight or any value therebetween; the amount of pure water is preferably 200-400 parts by weight, such as 200, 250, 300, 350, 400 parts by weight or any value therebetween. Controlling the amount of tea polyphenols within the above preferred range is more conducive to achieving the dispersion of graphene oxide (GO) and preventing GO from agglomerating.
[0023] In the present invention, the purpose of the first modification reaction is to graft the sulfonic acid group provided by the sulfonic acid source compound onto the graphene oxide, which can be specifically a modification reaction of 1 to 5 parts by weight of graphene oxide and 150 to 250 parts by weight of a sulfonic acid source compound solution under stirring, and after the stirring is completed, the graphene oxide powder modified with sulfonic acid groups is obtained by washing with pure water, filtering and drying. Wherein, the stirring time is not specifically limited, and can be a conventional choice in the art, preferably 20 to 28 hours, such as 20 hours, 22 hours, 24 hours, 26 hours, 28 hours or any value therebetween, which is more conducive to uniformly modifying the sulfonic acid group onto the graphene oxide without destroying the original structure of the graphene oxide.
[0024] In the present invention, the graphene oxide can be prepared by various methods in the prior art, or can be commercially available.
[0025] In the present invention, the purpose of the second modification reaction is to graft tea polyphenols onto sulfonic acid group-modified graphene oxide, which can be specifically a modification reaction of the sulfonic acid group-modified graphene oxide obtained in step S1 with 0.5 to 1.0 parts by weight of tea polyphenols and 200 to 400 parts by weight of pure water under stirring. Wherein, the stirring speed is preferably 4000 to 6000 rpm, such as 4000 rpm, 4500 rpm, 5000 rpm, 5500 rpm, 6000 rpm or any value therebetween, which is more conducive to uniformly and efficiently modifying tea polyphenols onto sulfonic acid group-modified graphene oxide; the stirring time is not specifically limited, and can be a conventional choice in the art, preferably 1 to 3 hours, such as 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours or any value therebetween. Preferably, step S2 may be: firstly mixing the sulfonic acid group-modified graphene oxide obtained in step S1 with 200 to 400 parts by weight of pure water and ultrasonically dispersing the mixture, then adding 0.5 to 1.0 parts by weight of tea polyphenols, and performing a second modification reaction under high-speed stirring at 4000 to 6000 rpm to obtain a graphene oxide dispersion.
[0026] The graphene oxide modified cement mortar provided by the present invention comprises a graphene oxide dispersion prepared by the above method, a water reducer, water, cement and sand, and optional additives and auxiliary materials. Wherein, the content of the graphene oxide dispersion is preferably 15 to 90 parts by weight, such as 15, 20, 30, 45, 60, 75, 80, 90 parts by weight or any value therebetween. The content of the water reducer is preferably 3 to 7 parts by weight, such as 3, 4, 5, 6, 7 parts by weight or any value therebetween. The content of the pure water is preferably 150 to 250 parts by weight, such as 150, 160, 175, 180, 190, 205, 220, 235, 250 parts by weight or any value therebetween. The content of the cement is preferably 300 to 500 parts by weight, such as 300, 350, 400, 450, 500 parts by weight or any value therebetween. The content of the sand is preferably 1000-1500 parts by weight, such as 1000, 1100, 1200, 1300, 1400, 1500 parts by weight or any value therebetween. The water reducer can be any existing water reducer, preferably a carboxylic acid water reducer. The additives and auxiliary materials can be any materials used in the preparation of cement mortar in the prior art, and the present invention does not specifically limit their types.
[0027] The graphene oxide modified cement mortar provided by the present invention is obtained by mixing the graphene oxide dispersion prepared by the above method, a water reducer, water, cement and sand, and optional additives and auxiliary materials. The order and method of mixing the above raw materials can be determined according to conventional selection. Preferably, the order and method of mixing the above raw materials can be: first disperse the graphene oxide dispersion prepared by the above method into water to obtain mixture I, then pre-mix cement and sand to obtain mixture II, and then mix and stir mixture I, water reducer, mixture II and optional additives and auxiliary materials to obtain graphene oxide modified cement mortar.
[0028] The present invention will be described in detail below through specific embodiments.
[0029] In the following preparation examples, embodiments and comparative examples, the parts of the raw materials involved are all parts by weight.
[0030] Sources of raw materials involved in the following preparation examples and embodiments: Graphene oxide powder was prepared by the Hummer method, flake graphite was oxidized, and then the graphene oxide was collected by filtration, followed by dialysis, and when the pH of the solution was neutral, the graphene oxide was collected for standby use; water reducer was purchased from Shanghai Chenqi Chemical Technology Co., Ltd., brand 540P.
[0031] Preparation Example 1 Preparation of graphene oxide dispersion
[0032] S1. Add 2 parts of graphene oxide powder into a 500 mL flask, then slowly pour 200 parts of concentrated sulfuric acid (mass percentage is 98wt%), stir at room temperature, and stir for 24 hours. After stirring, add 1000 parts of pure water for washing, then filter and dry to obtain sulfonic acid group-modified graphene oxide powder;
[0033] S2. Take the sulfonic acid group-modified graphene oxide powder prepared in step S1 and add it to a 500mL beaker. After adding 300 parts of pure water, place it in an ultrasonic machine for ultrasonication for 2 hours. Then, add 0.5 parts of tea polyphenols to the ultrasonicated solution and perform high-speed shear stirring at a speed of 5000rpm for 2 hours to obtain a graphene oxide dispersion.
[0034] Preparation Example 2 Preparation of graphene oxide dispersion
[0035] S1. Add 5 parts of graphene oxide powder into a 500 mL flask, then slowly pour 250 parts of concentrated sulfuric acid (mass percentage is 98wt%), stir at room temperature, and stir for 24 hours. After stirring, add 1000 parts of pure water for washing, then filter and dry to obtain sulfonic acid group-modified graphene oxide powder;
[0036] S2. Take the sulfonic acid group-modified graphene oxide powder prepared in step S1 and add it to a 500mL beaker. After adding 300 parts of pure water, place it in an ultrasonic machine for ultrasonication for 2 hours. Then, add 0.7 parts of tea polyphenols to the ultrasonicated solution and perform high-speed shear stirring at a speed of 5000rpm for 2 hours to obtain a graphene oxide dispersion.
[0037] Preparation Example 3 Preparation of graphene oxide dispersion
[0038] S1. Add 2 parts of graphene oxide powder into a 500 mL flask, then slowly pour 150 parts of concentrated sulfuric acid (mass percentage is 98wt%), stir at room temperature, and stir for 24 hours. After stirring, add 1000 parts of pure water for washing, then filter and dry to obtain sulfonic acid group-modified graphene oxide powder;
[0039] S2. Take the sulfonic acid group-modified graphene oxide powder prepared in step S1 and add it to a 500mL beaker. After adding 300 parts of pure water, place it in an ultrasonic machine for ultrasonication for 2 hours. Then, add 0.3 parts of tea polyphenols to the ultrasonicated solution and perform high-speed shear stirring at a speed of 5000rpm for 2 hours to obtain a graphene oxide dispersion.
[0040] Preparation Example 4 Preparation of graphene oxide dispersion
[0041] A graphene oxide dispersion was prepared according to the method of Preparation Example 1, except that the same amount of sodium dodecylbenzenesulfonate solution (mass percentage: 3wt%) was used instead of concentrated sulfuric acid (mass percentage: 98wt%), and the other conditions were the same as those in Preparation Example 1, thereby preparing a graphene oxide dispersion.
[0042] Comparative Preparation Example 1 Preparation of Reference Graphene Oxide Dispersion
[0043] 2 parts of graphene oxide powder were added to a 500 mL flask, and 300 parts of pure water were added, followed by ultrasonication in an ultrasonic machine for 2 hours, followed by high-speed shear stirring at a speed of 5000 rpm for 2 hours to obtain a reference graphene oxide dispersion.
[0044] Comparative Preparation Example 2 Preparation of Reference Graphene Oxide Dispersion
[0045] S1. Add 2 parts of graphene oxide powder into a 500 mL flask, then slowly pour 200 parts of concentrated sulfuric acid (mass percentage is 98wt%), stir at room temperature, and stir for 24 hours. After stirring, add 1000 parts of pure water for washing, then filter and dry to obtain sulfonic acid group-modified graphene oxide powder;
[0046] S2. Take the sulfonic acid group-modified graphene oxide powder prepared in step S1 and add it into a 500 mL beaker. After adding 300 parts of pure water, place it in an ultrasonic machine for ultrasonication for 2 hours to obtain a reference graphene oxide dispersion.
[0047] Comparative Preparation Example 3 Preparation of Reference Graphene Oxide Dispersion
[0048] Take 2 parts of graphene oxide powder and add them to a 500mL beaker. After adding 300 parts of pure water, place it in an ultrasonic machine for ultrasonication for 2 hours. Then, add 0.5 parts of tea polyphenols to the ultrasonicated solution and perform high-speed shear stirring at a speed of 5000rpm for 2 hours to obtain a reference graphene oxide dispersion.
[0049] Example 1 Graphene oxide modified cement mortar
[0050] 15 parts of the graphene oxide dispersion of Preparation Example 1 were ultrasonically dispersed in 250 parts of pure water for 0.2 h, and 5 parts of a water reducer were added to the dispersed solution. The mixture was then poured into a mixture of 400 parts of cement and 1200 parts of river sand, and stirred for 2 min to obtain a finished cement mortar.
[0051] Example 2 Graphene oxide modified cement mortar
[0052] 30 parts of the graphene oxide dispersion of Preparation Example 1 were ultrasonically dispersed in 235 parts of pure water for 0.2 h, and 5 parts of a water reducer were added to the dispersed solution. The mixture was then poured into a mixture of 400 parts of cement and 1200 parts of river sand, and stirred for 2 min to obtain a finished cement mortar.
[0053] Example 3 Graphene oxide modified cement mortar
[0054] 45 parts of the graphene oxide dispersion of Preparation Example 1 were ultrasonically dispersed in 220 parts of pure water for 0.2 h, and 5 parts of a water reducer were added to the dispersed solution. The mixture was then poured into a mixture of 400 parts of cement and 1200 parts of river sand, and stirred for 2 min to obtain a finished cement mortar.
[0055] Example 4 Graphene oxide modified cement mortar
[0056] 60 parts of the graphene oxide dispersion of Preparation Example 1 were ultrasonically dispersed in 205 parts of pure water for 0.2 h, and 5 parts of a water reducer were added to the dispersed solution. The mixture was then poured into a mixture of 400 parts of cement and 1200 parts of river sand, and stirred for 2 min to obtain a finished cement mortar.
[0057] Example 5 Graphene oxide modified cement mortar
[0058] 75 parts of the graphene oxide dispersion of Preparation Example 1 were ultrasonically dispersed in 190 parts of pure water for 0.2 h, and 5 parts of a water reducer were added to the dispersed solution. The mixture was then poured into a mixture of 400 parts of cement and 1200 parts of river sand, and stirred for 2 min to obtain a finished cement mortar.
[0059] Example 6 Graphene oxide modified cement mortar
[0060] 90 parts of the graphene oxide dispersion of Preparation Example 1 were ultrasonically dispersed in 175 parts of pure water for 0.2 h, and 5 parts of a water reducer were added to the dispersed solution. The mixture was then poured into a mixture of 400 parts of cement and 1200 parts of river sand, and stirred for 2 min to obtain a finished cement mortar.
[0061] Example 7 Graphene oxide modified cement mortar
[0062] Graphene oxide modified cement mortar was prepared according to the method of Example 4, except that the graphene oxide dispersion of Preparation Example 2 was used in the same weight portion instead of the graphene oxide dispersion of Preparation Example 1, and the other conditions were the same as those of Example 4, thereby obtaining a finished cement mortar.
[0063] Example 8 Graphene oxide modified cement mortar
[0064] Graphene oxide modified cement mortar was prepared according to the method of Example 4, except that the graphene oxide dispersion of Preparation Example 3 was used in the same weight portion instead of the graphene oxide dispersion of Preparation Example 1, and the other conditions were the same as those of Example 4, thereby obtaining a finished cement mortar.
[0065] Example 9 Graphene oxide modified cement mortar
[0066] Graphene oxide modified cement mortar was prepared according to the method of Example 4, except that the graphene oxide dispersion of Preparation Example 4 was used in the same weight portion instead of the graphene oxide dispersion of Preparation Example 1, and the other conditions were the same as those of Example 4, thereby obtaining a finished cement mortar.
[0067] Comparative Example 1: Cement mortar modified with graphene oxide
[0068] A reference graphene oxide-modified cement mortar was prepared according to the method of Example 4, except that the graphene oxide dispersion of Comparative Preparation Example 1 was used in the same weight portion instead of the graphene oxide dispersion of Preparation Example 1, and the other conditions were the same as those of Example 4, thereby obtaining a finished cement mortar.
[0069] Comparative Example 2: Cement mortar modified with graphene oxide
[0070] A reference graphene oxide-modified cement mortar was prepared according to the method of Example 4, except that the graphene oxide dispersion of Comparative Preparation Example 2 was used instead of the graphene oxide dispersion of Preparation Example 1 in equal parts by weight, and the other conditions were the same as those of Example 4, thereby obtaining a finished cement mortar.
[0071] Comparative Example 3: Cement mortar modified with graphene oxide
[0072] A reference graphene oxide-modified cement mortar was prepared according to the method of Example 4, except that the graphene oxide dispersion of Comparative Preparation Example 3 was used in place of the graphene oxide dispersion of Preparation Example 1 in equal parts by weight, and the remaining conditions were the same as those of Example 4, thereby obtaining a finished cement mortar.
[0073] Test Case
[0074] The graphene oxide modified cement mortar prepared in the above examples and comparative examples was tested for fluidity, compressive strength and flexural strength according to the following methods, and the results are shown in Table 1.
[0075] (1) Fluidity test: The fluidity was tested according to the method in GB / T8077-2000 "Test method for homogeneity of concrete admixtures". The graphene oxide-modified cement mortar prepared in the above embodiment and comparative example was injected into a truncated cone circular mold and filled. The truncated cone circular mold was lifted and the maximum diameter of the cement mortar flowing freely on a glass plane was measured.
[0076] (2) Compressive strength and flexural strength test: The cement mortars prepared in the examples and comparative examples were subjected to compressive strength and flexural strength tests according to the method in GB / T50080-2002. The results are shown in Table 1.
[0077] Table 1
[0078]
[0079] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. A method for preparing a graphene oxide dispersion, It is characterized in that The preparation method comprises: S1. performing a first modification reaction of graphene oxide and a sulfonic acid source compound in a first solution to obtain sulfonic acid group-modified graphene oxide; S2. The sulfonic acid group-modified graphene oxide obtained in step S1 is subjected to a second modification reaction with tea polyphenols in a second solution to obtain a graphene oxide dispersion.
2. The method for preparing a graphene oxide dispersion according to claim 1, It is characterized in that In step S1, the sulfonic acid source compound is used in the form of a sulfonic acid source compound solution; Optionally, in step S1, the amount of graphene oxide used is 1 to 5 parts by weight, and the amount of the sulfonic acid source compound solution used is 150 to 250 parts by weight.
3. The method for preparing the graphene oxide dispersion according to claim 1, It is characterized in that In step S2, the amount of tea polyphenols used is 0.3-0.7 parts by weight, and the amount of the second solution used is 200-400 parts by weight.
4. The method for preparing a graphene oxide dispersion according to any one of claims 1 to 3, It is characterized in that The first modification reaction is a reaction of graphene oxide with a sulfonic acid source compound and a first solution under stirring; Optionally, the stirring time is 20 to 28 hours.
5. The method for preparing a graphene oxide dispersion according to any one of claims 1 to 3, It is characterized in that The second modification reaction is a reaction of the sulfonic acid group-modified graphene oxide obtained in step S1 with tea polyphenols and the second solution under stirring; Optionally, the stirring speed is 4000-6000 rpm, and the stirring time is 1-3 hours.
6. The method for preparing a graphene oxide dispersion according to any one of claims 1 to 3, It is characterized in that The sulfonic acid source compound is selected from at least one of sulfuric acid, sulfurous acid, sodium wood sulfonate, and sodium dodecylbenzene sulfonate.
7. A graphene oxide dispersion prepared by the method for preparing a graphene oxide dispersion according to any one of claims 1 to 6.
8. A cement mortar modified with graphene oxide, It is characterized in that The cement mortar contains the graphene oxide dispersion according to claim 7, a water reducer, water, cement and sand, and optional additives and auxiliary materials.
9. The graphene oxide modified cement mortar according to claim 8, It is characterized in that The content of the graphene oxide dispersion is 15 to 90 parts by weight, the content of the water reducer is 3 to 7 parts by weight, the content of water is 150 to 250 parts by weight, the content of cement is 300 to 500 parts by weight, the content of sand is 1000 to 1500 parts by weight, the content of the auxiliary agent is 0.6 to 2.5 parts by weight, and the content of the auxiliary material is 1.2 to 3.0 parts by weight.
10. Use of the graphene oxide dispersion according to claim 7 and / or the graphene oxide-modified cement mortar according to claim 8 or 9 in the field of building materials.
Citation Information
Patent Citations
Method for preparation of graphene through synergistic action of ascorbic acid / tea polyphenol
CN107161984A
Preparation method for highly-dispersed few-layer graphene
CN110117002A
Graphene aqueous dispersion liquid, graphene concrete and preparation methods of graphene aqueous dispersion liquid and graphene concrete
CN110498634A
Sulfonic group modified graphene, and preparation method and application thereof in water-based epoxy coating
CN110655071A
Graphene oxide compounded cement mortar and preparation method thereof
CN110857246A