Powder coating and sintering method of ceramic substrate and ceramic substrate

By using high-purity and appropriate particle size separator powder during the sintering process of the ceramic substrate and sintering under an inert atmosphere, the problem of pockmarking of ceramic substrates is solved, and the sintering efficiency and finished product quality are improved.

CN118993746APending Publication Date: 2024-11-22GUANGDONG HUANBO NEW MATERIAL CO LTD +1

Patent Information

Application Number
CN202411033559.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Ceramic substrates are prone to pitting during sintering, resulting in poor quality of finished products, and it is difficult for the prior art to effectively solve this problem.

Method used

The separator powder with a purity of ≥99.99% was used, with a particle size range of 1 μm to 100 μm. It was laid between the ceramic blanks and sintered in combination with an inert atmosphere to reduce the reaction risk between the separator powder and the ceramic blanks.

Benefits of technology

It significantly reduces the occurrence of pitting on the surface of the ceramic substrate, improves the sintering efficiency and the quality of the finished product, and ensures the compactness and stability of the ceramic substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993746A_ABST
    Figure CN118993746A_ABST
Patent Text Reader

Abstract

The invention discloses a powder coating sintering method of a ceramic substrate and the ceramic substrate, and belongs to the technical field of ceramic substrate preparation processes. According to the method, the ceramic substrate is prepared through the steps of powder coating, degreasing and sintering, the adhesion isolation powder with the purity larger than or equal to 99.99% and the particle size ranging from 1 micrometer to 100 micrometers is selected in the powder coating step, the purity of the adhesion isolation powder is improved, and the risk that pits appear on the finished ceramic substrate due to the fact that the adhesion isolation powder reacts with a ceramic biscuit in the sintering process is reduced; sintering treatment is carried out in an inert atmosphere, so that pocking marks on the finished ceramic substrate caused by reaction of the isolation powder, floating dust and the product can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic substrate preparation technology, and in particular to a powder coating and sintering method for a ceramic substrate and a ceramic substrate. Background Art

[0002] In recent years, with the vigorous development of the microelectronics packaging industry, electronic packaging technology has developed in the direction of miniaturization, high density, multi-power and high reliability. Electronic packaging materials have gradually become an industrial field with high technology content, high economic benefits and important status. At present, the commonly used substrate materials mainly include plastic substrates, metal substrates, ceramic substrates and composite substrates. The ultra-thin composite substrate made of advanced ceramic materials has excellent electrical insulation properties, high thermal conductivity, excellent soft soldering and high adhesion strength. It can be etched with various patterns like PCB boards and has a large current carrying capacity. Ceramic substrates are widely used in high-power power semiconductor modules, power control circuits, automotive electronics, aerospace and military electronic components, solar panel components and other fields because of their much better heat dissipation performance, current carrying capacity, insulation, thermal expansion coefficient, etc. than ordinary glass fiber PCB boards. Ceramic substrate manufacturers have increased their investment and improved their R&D capabilities, but their R&D capabilities for high-end products still need to be improved. For example, in large-scale production processes, in order to improve sintering efficiency, multiple ceramic blanks are usually stacked and then collectively degreased and sintered. In order to make the resulting ceramic substrates easy to separate from each other, a layer of isolation powder needs to be laid between the ceramic blanks. However, during the sintering process, the isolation powder and the ceramic blanks are prone to react, resulting in pitting on the surface of the ceramic substrate. In addition, during the sintering process, the ceramic blanks are prone to react with the isolation powder and dust in the air, resulting in pitting on the surface of the ceramic substrate. Summary of the invention

[0003] The main purpose of the present invention is to provide a powder coating and sintering method for a ceramic substrate and a ceramic substrate, so as to solve the technical problem that pitting is easy to occur on the ceramic substrate.

[0004] To achieve the above object, the present invention provides a powder coating and sintering method for a ceramic substrate, comprising the following steps:

[0005] Powder coating: placing two or more layers of ceramic blanks on a firing plate, and laying a layer of insulating powder between any two of the ceramic blanks to obtain a powder-coated ceramic blank, wherein the purity of the insulating powder is ≥99.99%, and the particle size of the insulating powder is in the range of 1 μm to 100 μm;

[0006] Degreasing: degreasing the powder-coated ceramic blank to obtain a degreased ceramic blank;

[0007] Sintering: The degreased ceramic green body is sintered in an inert atmosphere to obtain the ceramic substrate.

[0008] In some embodiments of the present invention, the anti-sticking powder includes aluminum oxide.

[0009] In some embodiments of the present invention, a layer of the isolation powder has a thickness ranging from 1 μm to 100 μm.

[0010] In some embodiments of the present invention, the inert atmosphere includes a nitrogen atmosphere and / or an argon atmosphere.

[0011] In some embodiments of the present invention, in the degreasing step, the temperature is raised to 400° C. to 800° C. and then the temperature is kept warm for 4 to 6 hours.

[0012] In some embodiments of the present invention, in the sintering step, the sintering temperature ranges from 1450°C to 1600°C.

[0013] In some embodiments of the present invention, the method for preparing the ceramic blank comprises the following steps:

[0014] Preparation of slurry: mixing alumina powder and a dispersant in an organic solvent, and then adding a plasticizer and a binder to obtain a slurry;

[0015] Casting: Casting the slurry into a green porcelain tape;

[0016] Laminated isostatic pressing: The green porcelain tape is laminated and isostatically pressed to obtain a ceramic blank.

[0017] In some embodiments of the present invention, the purity of the aluminum oxide powder is 99.6% to 99.999%;

[0018] And / or, the particle size D50 of the alumina powder is 0.5 μm to 1.0 μm.

[0019] In some embodiments of the present invention, in the step of preparing the slurry, alumina powder, a dispersant and a sintering aid are mixed in an organic solvent.

[0020] The present invention also provides a ceramic substrate prepared by the powder coating and sintering method of the ceramic substrate as described above.

[0021] The beneficial effects that can be achieved by the present invention are:

[0022] The present invention adds a powder coating step in the process of preparing a ceramic substrate, thereby improving the sintering efficiency. At the same time, in the powder coating step, a separation powder with a purity of ≥99.99% is applied to the surface of the ceramic blank away from the sintering plate, thereby improving the purity of the separation powder and reducing the risk of pitting on the finished ceramic substrate caused by the separation powder reacting with the ceramic blank during the sintering process. In addition, the particle size range of the separation powder is controlled to be 1 μm to 100 μm, thereby reducing the separation powder from reacting with the ceramic blank due to its small particle size and strong surface activity, thereby reducing the risk of pitting on the finished ceramic substrate, and preventing pits from forming on the surface of the ceramic substrate due to the excessive particle size of the separation powder. Furthermore, the present invention also performs sintering treatment in an inert atmosphere, thereby alleviating the problem of pitting on the finished ceramic substrate caused by the separation powder and floating dust reacting with the ceramic blank. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0024] Figure 1 The figure is a schematic flow chart of a powder coating and sintering method for a ceramic substrate according to an embodiment of the present invention.

[0025] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0026] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0029] In the process of preparing ceramic substrates, the raw material alumina powder has a high purity, and it is difficult to produce a liquid phase during the sintering process, which easily leads to the formation of closed pores. It is also difficult to remove organic matter, thus forming closed pores during the sintering process, which causes gray spots to appear on the ceramic substrate.

[0030] In view of this, the present invention provides a ceramic substrate and a preparation method thereof, referring to Figure 1 , the preparation method comprises the following steps:

[0031] S10, powder coating: placing two or more layers of ceramic blanks on a firing plate, and laying a layer of insulating powder between any two of the ceramic blanks to obtain a powder-coated ceramic blank, wherein the purity of the insulating powder is ≥99.99%, and the particle size of the insulating powder is in the range of 1 μm to 100 μm;

[0032] S20, degreasing: degreasing the powder-coated ceramic blank in an inert atmosphere to obtain a degreased ceramic blank;

[0033] S30, sintering: sintering the degreased ceramic green blank to obtain the anti-pitting ceramic substrate.

[0034] In order to improve the sintering efficiency, the present invention stacks multiple layers of ceramic blanks and then performs degreasing and sintering treatments. However, the ceramic blanks are in direct contact with each other, and adverse effects such as bonding are likely to occur during the subsequent degreasing and sintering processes. Therefore, the present invention provides a layer of insulating powder between any two layers of ceramic blanks, and the increase of insulating powder will cause new problems. For example, during the sintering process, the insulating powder is likely to react with the ceramic blanks to cause pitting on the surface of the ceramic substrate. Therefore, the present invention selects insulating powder with a purity of ≥99.99% and a particle size range of 1μm to 100μm, which improves the purity of the insulating powder and reduces the risk of insulating powder reacting with the ceramic blanks during the sintering process due to excessive impurities, resulting in pitting on the finished ceramic substrate. At the same time, controlling the particle size range of the insulating powder to 1μm to 100μm not only reduces the insulating powder due to too small a particle size and too strong a surface activity, which is easy to react with the ceramic blanks to cause pitting on the finished ceramic substrate, but also does not cause pits on the surface of the ceramic substrate due to the excessively large particle size of the insulating powder.

[0035] It can be understood that the purity of the isolation powder can be 99.99%, 99.995%, 99.999%, etc. ≥99.99% purity, and the particle size can be 1μm, 5μm, 10μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 70μm, 90μm, 100μm, etc., any value in the range of 1μm to 100μm.

[0036] In some embodiments, the isolating powder includes aluminum oxide, which is less likely to react with the ceramic green body to damage the quality of the ceramic substrate.

[0037] In some embodiments, the thickness of a layer of insulating powder laid between any two layers of ceramic blanks is 1 μm to 100 μm, and can be any value in the range of 1 μm to 100 μm, such as 1 μm, 5 μm, 10 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 70 μm, 90 μm, 100 μm, etc.

[0038] In the degreasing step, organic matter in the ceramic green body can be removed, reducing the problem of gray spots on the finished ceramic substrate caused by residual organic matter.

[0039] In some embodiments of the degreasing step, degreasing gas is introduced into the degreasing step to degrease the powder-coated ceramic green body.

[0040] In some embodiments of the degreasing step, the degreasing gas introduced includes air and / or nitrogen, and the air and / or nitrogen react with organic matter in the ceramic blank to reduce the residual organic matter and reduce the gray spots in the finished ceramic substrate.

[0041] In some embodiments of the degreasing step, degreasing gas is introduced at an air flow rate of 20L / min to 50L / min, and the ceramic blank is degreased at a heating rate of 0.2°C / min to 0.5°C / min to obtain a degreased ceramic blank. For example, the air flow rate can be any value in the range of 20L / min to 50L / min, such as 20L / min, 25L / min, 30L / min, 35L / min, 40L / min, 45L / min, 50L / min, and the heating rate can be any value in the range of 0.2°C / min to 0.5°C / min, such as 0.2°C / min, 0.3°C / min, 0.4°C / min, 0.5°C / min. Under the above air flow rate and heating rate conditions, it is beneficial to discharge organic matter inside the ceramic substrate, reduce the generation of closed pores in the ceramic blank during the sintering process due to organic residue, and then affect the quality of the ceramic substrate, such as the appearance of defects such as gray spots.

[0042] In some embodiments of the degreasing step, the temperature is raised from room temperature 25°C to 30°C at a heating rate of 0.2°C / min to 0.5°C / min to 400°C to 800°C, and then kept warm. The holding time can be 4h to 6h. The degreasing treatment is carried out at 400°C to 800°C, which is conducive to promoting the discharge of organic matter and preventing excessive organic matter from remaining and causing gray spots on the ceramic substrate due to the formation of closed pores. In this embodiment, the temperature can be raised to any temperature in the range of 400°C to 800°C, such as 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, etc., and the holding time can be any value in the range of 4h to 6h, such as 4h, 4.5h, 5h, 5.5h, 6h, etc.

[0043] In the sintering step, the ceramic blank can be formed into a ceramic substrate. During the sintering process, the ceramic blank is easy to react with the isolation powder and the dust in the air in the air atmosphere to cause pitting on the surface of the ceramic substrate. Therefore, the sintering of the present invention is carried out in an inert atmosphere, which is conducive to reducing the risk of the ceramic blank easily reacting with the isolation powder and the dust in the air in the air atmosphere to cause pitting on the surface of the ceramic substrate.

[0044] In some embodiments of the sintering step, the inert atmosphere includes a nitrogen atmosphere and / or an argon atmosphere. For example, nitrogen and / or argon are introduced before sintering to obtain a nitrogen atmosphere and / or an argon atmosphere.

[0045] In some embodiments of the sintering step, the sintering temperature ranges from 1450°C to 1600°C, and can be any value in the range of 1450°C to 1600°C, such as 1450°C, 1500°C, 1520°C, 1550°C, 1580°C, 1600°C, etc. Under the above sintering temperature conditions, it is beneficial to promote the sintering molding of the ceramic substrate.

[0046] In some embodiments of the sintering step, the sintering heating rate is 0.1°C / min to 0.5°C / min, for example, it can be any value in the range of 0.1°C / min to 0.5°C / min, such as 0.1°C / min, 0.2°C / min, 0.3°C / min, 0.4°C / min, 0.5°C / min, etc. Under the above sintering heating rate conditions, it is beneficial to the sintering molding of the ceramic substrate, and the heating rate is slow, which is beneficial to promote the discharge of gas in the degreased ceramic blank and reduce the generation of pinholes in the finished ceramic substrate.

[0047] In some embodiments, the temperature is lowered after sintering is completed, and the cooling rate is 0.1°C / min to 0.5°C / min, for example, it can be any value in the range of 0.1°C / min to 0.5°C / min, such as 0.1°C / min, 0.2°C / min, 0.3°C / min, 0.4°C / min, 0.5°C / min, etc. Under the above cooling rate conditions, the closed bubbles in the degreased ceramic blank can be caused to collapse in time, thereby reducing the generation of pinholes in the finished ceramic substrate.

[0048] In some embodiments, the method for preparing a ceramic blank comprises the following steps:

[0049] Preparation of slurry: mixing alumina powder and a dispersant in an organic solvent, and then adding a plasticizer and a binder to obtain a slurry;

[0050] Casting: Casting the slurry into a green porcelain tape;

[0051] Laminated isostatic pressing: The green porcelain tape is laminated and isostatically pressed to obtain a ceramic blank.

[0052] In some embodiments, the powder coating and sintering method of the ceramic substrate of the present invention comprises the following steps:

[0053] Preparation of slurry: mixing alumina powder and a dispersant in an organic solvent, and then adding a plasticizer and a binder to obtain a slurry;

[0054] Casting: Casting the slurry into a green porcelain tape;

[0055] Laminated isostatic pressing: The green porcelain tape is laminated and isostatically pressed to obtain a ceramic blank.

[0056] Powder coating: placing two or more layers of ceramic blanks on a firing plate, and laying a layer of insulating powder between any two of the ceramic blanks to obtain a powder-coated ceramic blank, wherein the purity of the insulating powder is ≥99.99%, and the particle size of the insulating powder is in the range of 1 μm to 100 μm;

[0057] Degreasing: degreasing the powder-coated ceramic green blank in an inert atmosphere to obtain a degreased ceramic green blank;

[0058] Sintering: Sintering the degreased ceramic green blank to obtain the anti-pitting ceramic substrate.

[0059] In some embodiments, the particle size D50 of the alumina powder is 0.5 μm to 1.0 μm, and can be any value in the range of 0.5 μm to 1.0 μm, such as 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, etc. The alumina powder under the above particle size range conditions is conducive to promoting the dispersion of the alumina powder and sintering to obtain a dense, structurally stable, electromechanically stable, smooth surface, and less gray spots and pitting ceramic substrate.

[0060] In some embodiments, the purity of the aluminum oxide powder is 99.6% to 99.999%. The purity of aluminum oxide is relatively high, and the content of combustible impurities and volatile impurities therein is relatively low, which can reduce the occurrence of pinholes in the ceramic substrate caused by excessive gas generated by combustible gas and volatile impurities during the sintering process. In this embodiment, although increasing the purity of aluminum oxide powder can reduce the occurrence of pinholes, the purity of aluminum oxide powder reaches 99.9% or more, and the high purity will face the problem of difficulty in forming liquid during the sintering process, resulting in the formation of closed pores, thereby causing the formation of gray spots on the finished ceramic substrate.

[0061] Therefore, in some embodiments, in the step of preparing the slurry, in the step of mixing the alumina powder and the dispersant in the organic solvent, a sintering aid can also be added for mixing. The sintering aid can form a liquid phase during the sintering process and has fluidity, and can effectively fill the pores, gaps or defects generated during the sintering process, thereby reducing the generation of closed pores during the sintering process and alleviating the problem of gray spots in the finished ceramic substrate. In this embodiment, alumina powder with a high purity of 99.6% to 99.999% can be used as a raw material to obtain a ceramic substrate with a stable structure, fewer closed pores, and fewer pinholes and gray spots.

[0062] In some embodiments, the sintering aid includes magnesium oxide, which can become a fluid liquid during high-temperature sintering, effectively filling the pores, voids or defects generated during the sintering process, reducing the generation of closed pores in the ceramic substrate, thereby reducing gray spots.

[0063] In some embodiments, the particle size range of the sintering aid is 0.5μm to 1.0μm, and can be any value in the range of 0.5μm to 1.0μm, such as 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm, etc. The sintering aid is conducive to matching with the alumina powder under the above particle size range conditions, and is easy to form a liquid with fluidity during high-temperature sintering, and effectively fills the pores, voids or defects generated during the sintering process, which is conducive to sintering to obtain a ceramic substrate with uniform structure, while reducing the generation of closed pores to reduce gray spots in the finished ceramic substrate.

[0064] In some embodiments, the particle size range of the sintering aid is 0.5μm to 1.0μm, and can be any value in the range of 0.5μm to 1.0μm, such as 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm, etc. The sintering aid is conducive to matching with the alumina powder under the above particle size range conditions, and is easy to form a liquid with fluidity during high-temperature sintering, and effectively fills the pores, voids or defects generated during the sintering process, which is conducive to sintering to obtain a ceramic substrate with uniform structure, while reducing the generation of closed pores to reduce gray spots in the finished ceramic substrate.

[0065] In the present invention, the organic solvent plays the role of dissolving the alumina powder and mixing various raw materials.

[0066] In some embodiments, the organic solvent includes an ester compound and an alcohol compound, wherein the ester compound includes at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate; and / or the alcohol compound includes at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol.

[0067] In some embodiments, the mass ratio of alcohol compounds to ester compounds in the organic solvent is (7-9):(1-3), which can be 7:1, 7:2, 7:3, 8:1, 8:2, 8:3, 9:1, 9:2, 9:3.

[0068] In some embodiments, the dispersant includes triolein. Using triolein as a dispersant is beneficial to promoting uniform dispersion of the aluminum oxide powder.

[0069] In the present invention, the plasticizer plays a role in enhancing the strength and toughness of the ceramic substrate.

[0070] In some embodiments, the plasticizer includes at least one of dibutyl phthalate and polyethylene glycol.

[0071] In the present invention, the binder can strengthen the bonding force between various raw materials, which is beneficial to obtain a ceramic substrate with a stable structure.

[0072] In some embodiments, the binder includes polyvinyl butyral.

[0073] In some embodiments, the ceramic substrate includes the following components, calculated by weight percentage: aluminum oxide powder: 40% to 60%; organic solvent: 30% to 45%; dispersant: 0.5% to 3%; plasticizer: 4.5% to 10%; binder: 3.5% to 10%; sintering aid: 0.2% to 1.2%. For example, the aluminum oxide powder can be 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, etc., and the organic solvent can be 30%, 35%, 40%, 45%, etc. % or any value in the range of 30% to 45%; the dispersant can be any value in the range of 0.5% to 3% such as 0.5%, 1%, 2%, 3%, etc.; the plasticizer can be any value in the range of 4.5% to 10% such as 4.5%, 5%, 6%, 7%, 8%, 9%, 10%, etc.; the binder can be any value in the range of 3.5% to 10% such as 3.5%, 5%, 7%, 8%, 9%, 10%, etc.; the sintering aid can be any value in the range of 0.2% to 1.2% such as 0.2%.

[0074] In the step of preparing the slurry, the alumina powder and the dispersant are first dispersed in an organic solvent for dispersion, which can enhance the dispersion effect of the alumina powder in the entire slurry system, thereby preparing a ceramic substrate with a stable structure.

[0075] In some embodiments, after the alumina powder and the dispersant are dispersed in the organic solvent, they can be mixed by ball milling for 20 to 30 hours, for example, 20 hours, 24 hours, 28 hours, 30 hours, etc., to promote uniform dispersion of the alumina powder.

[0076] In some embodiments, after adding the thickener, the binder and the sintering aid, the mixture may be further ball-milled in a ball mill to obtain a slurry.

[0077] In the casting step, the thickness of the green porcelain tape can be controlled according to actual needs. In some embodiments, the thickness of the green porcelain tape ranges from 30μm to 60μm, and can be 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, etc., in the range of 30μm to 60μm.

[0078] The laminated isostatic pressing treatment is beneficial for obtaining a high-density and uniform ceramic green body, which reduces the shrinkage of the ceramic green body during the subsequent sintering process and is not prone to deformation.

[0079] In some steps of laminated isostatic pressing, the temperature range of isostatic pressing treatment is 50℃~80℃, and can be any value within the range of 50℃~80℃, such as 50℃, 60℃, 70℃, 80℃, etc. Within the above temperature range of isostatic pressing treatment, it is beneficial to obtain a ceramic green body with high density and uniformity, and the ceramic green body is not prone to shrinkage and deformation.

[0080] In some steps of laminated isostatic pressing, the pressure range of isostatic pressing treatment is 50MPa~100MPa, and can be any value in the range of 50MPa~100MPa, such as 50MPa, 60MPa, 70MPa, 80MPa, 90MPa, 100MPa, etc. Under the above isostatic pressing treatment pressure conditions, a high-density ceramic green body can be obtained, and it is not easy to cause deformation of the ceramic green body.

[0081] In some steps of laminated isostatic pressing, the holding time of the isostatic pressing treatment is 5 minutes to 20 minutes, and can be any value in the range of 5 minutes to 20 minutes, such as 5 minutes, 8 minutes, 10 minutes, 12 minutes, 15 minutes, 18 minutes, 20 minutes, etc. Under the above holding time range conditions, a high-density ceramic green body can be obtained, and it is not easy to cause deformation of the ceramic green body.

[0082] The ceramic substrate prepared by the powder coating and sintering method of the ceramic substrate as described above has good quality, a firm and stable structure, high density and fewer pits.

[0083] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following specific embodiments are only used to explain the present invention, and are not used to limit the present invention.

[0084] Example 1

[0085] Embodiment 1 A powder coating and sintering method for a ceramic substrate comprises the following steps:

[0086] Preparation of slurry: Weigh 1000 g of alumina powder with a particle size D50 of 0.6 μm and a purity of 99.98%, dissolve it in a mixed solvent of 560 g of ethyl acetate and 240 g of ethanol, then add 20 g of dispersant triolein and 5 g of sintering aid magnesium oxide with a particle size D50 of 0.5 μm, mix by ball milling for 24 h, then add 100 g of plasticizer dibutyl phthalate and 80 g of binder polyvinyl butyral, and continue mixing for 24 h to obtain slurry;

[0087] Tape casting: The slurry is cast into a green porcelain tape with a thickness of 60 μm;

[0088] Laminated isostatic pressing: laminate the green porcelain tape obtained after tape casting to the required thickness, evacuate the green porcelain tape by isostatic pressing, put the product into the isostatic pressing machine after evacuation, set the temperature to 60°C, the pressure to 80MPa, and the holding time to 10min to obtain the ceramic green body;

[0089] Powder coating: Place the first layer of ceramic blank on the firing plate, and evenly coat the surface of the ceramic blank with a layer of 99.995% purity and 50μm particle size of isolation powder, then place the second layer of ceramic blank on the surface of the isolation powder, and then evenly coat the surface of the second layer of ceramic blank with a layer of 99.995% purity and 50μm particle size of isolation powder, and repeat this process to obtain the required number of layers of powdered ceramic blanks, so that there is a layer of isolation powder between any two layers of ceramic blanks;

[0090] Degreasing: introducing a mixed gas of degreasing air and nitrogen at an air flow rate of 30 L / min, heating the mixture to 500° C. at a heating rate of 0.2° C. / min, and then maintaining the temperature for 2 hours to degrease the ceramic blank to obtain a degreased ceramic blank;

[0091] Sintering: In a nitrogen atmosphere, the degreased ceramic green body was sintered at a heating rate of 0.1°C / min to 1530°C, then cooled to 1000°C at a cooling rate of 0.1°C / min, kept at that temperature for 4 hours, and naturally cooled to room temperature to obtain a ceramic substrate.

[0092] Example 2 to Example 4

[0093] Examples 2 to 4 all refer to the preparation method of Example 1 to prepare ceramic substrates, except that the particle size and purity of the adhesive powder in Examples 2 to 4 are different, as shown in Table 1 for details.

[0094] Comparative Example 1

[0095] Comparative Example 1 A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the sintering atmosphere was air, as shown in Table 1.

[0096] Comparative Example 2

[0097] Comparative Example 2 A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the purity of the isolation powder was 99.92%, as shown in Table 1.

[0098] Comparative Example 3

[0099] Comparative Example 3 A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the particle size of the adhesive isolation powder in Comparative Example 3 was 0.1 μm, as shown in Table 1 for details.

[0100] Comparative Example 4

[0101] Comparative Example 4 A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the particle size of the insulating powder in Comparative Example 4 was 150 μm, as shown in Table 1.

[0102] Performance Testing

[0103] The number of pits and depressions on the surface of the ceramic substrates prepared in the examples and comparative examples were observed.

[0104] Table 1

[0105] Experimental Group Sintering atmosphere Purity of adhesive powder Particle size of anti-adhesive powder Number of pitting Number of pits Example 1 Argon 99.995% 50μm 0 0 Example 2 Nitrogen 99.991% 50μm 0 0 Example 3 Argon 99.995% 30μm 0 0 Example 4 Argon 99.995% 60μm 0 0 Comparative Example 1 Air 99.995% 50μm 12 0 Comparative Example 2 Nitrogen 99.92% 50μm 5 0 Comparative Example 3 Nitrogen 99.995% 0.1μm 3 0 Comparative Example 4 Nitrogen 99.995% 150μm 0 8

[0106] It can be known from Examples 1 to 4 that the ceramic substrates prepared by the preparation method of the present invention in Examples 1 to 4 are sintered in an inert atmosphere, which can reduce the reaction between isolation powder and floating dust and the product to cause pitting on the finished ceramic substrate, and the powder coating treatment is completed using isolation powder with a purity of ≥99.99% and a particle size of 1μm to 100μm, which improves the purity of the isolation powder and reduces the risk of the isolation powder reacting with the ceramic blank during the sintering process to cause pitting on the finished ceramic substrate. The particle size range of the isolation powder is 1μm to 100μm, which not only alleviates the problem that the isolation powder is too small in particle size and too strong in surface activity to easily react with the ceramic blank to cause pitting on the finished ceramic substrate, but also prevents pits from forming on the surface of the ceramic substrate due to the large particle size of the isolation powder.

[0107] In Comparative Example 1, the sintering atmosphere is air, and the ceramic green body easily reacts with the isolation powder and the dust floating in the air, resulting in pitting on the surface of the ceramic substrate, and the number of pitting is 12.

[0108] The purity of the insulating powder in Comparative Example 2 is 99.92%, and it contains a lot of impurities. It is easy to react with the ceramic green body during the sintering process to cause pitting on the surface of the ceramic substrate. The number of pitting is 5.

[0109] The particle size of the insulating powder in Comparative Example 3 is 0.1 μm, which is too small, has a large specific surface area, and has a large surface activity. During the sintering process, it is easy to react with the ceramic green body to cause pitting on the surface of the ceramic substrate. The number of pitting is 3.

[0110] The particle size of the anti-sticking powder in Comparative Example 4 is 150 μm, which is too large, resulting in 8 pits on the ceramic substrate.

[0111] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A powder coating and sintering method for a ceramic substrate, characterized in that: The following steps are involved: Powder coating: placing two or more layers of ceramic blanks on a firing plate, and laying a layer of insulating powder between any two of the ceramic blanks to obtain a powder-coated ceramic blank, wherein the purity of the insulating powder is ≥99.99%, and the particle size of the insulating powder is in the range of 1 μm to 100 μm; Degreasing: degreasing the powder-coated ceramic blank to obtain a degreased ceramic blank; Sintering: The degreased ceramic green body is sintered in an inert atmosphere to obtain the ceramic substrate.

2. The powder coating and sintering method of a ceramic substrate according to claim 1, characterized in that: The anti-sticking powder includes aluminum oxide.

3. The powder coating and sintering method of a ceramic substrate according to claim 1, characterized in that: The thickness of a layer of the isolating powder is in the range of 1 μm to 100 μm.

4. The powder coating and sintering method of a ceramic substrate according to claim 1, characterized in that: The inert atmosphere includes a nitrogen atmosphere and / or an argon atmosphere.

5. The powder coating and sintering method of a ceramic substrate according to claim 1, characterized in that: In the degreasing step, the temperature is raised to 400° C. to 800° C. and then heat-insulated for 4 to 6 hours.

6. The powder coating and sintering method of a ceramic substrate according to claim 1, characterized in that: In the sintering step, the sintering temperature ranges from 1450°C to 1600°C.

7. The powder coating and sintering method of a ceramic substrate according to any one of claims 1 to 6, characterized in that: The method for preparing the ceramic blank comprises the following steps: Preparation of slurry: mixing alumina powder and a dispersant in an organic solvent, and then adding a plasticizer and a binder to obtain a slurry; Casting: Casting the slurry into a green porcelain tape; Laminated isostatic pressing: The green porcelain tape is laminated and isostatically pressed to obtain a ceramic blank.

8. The powder coating and sintering method of a ceramic substrate according to claim 7, characterized in that: The purity of the aluminum oxide powder is 99.6% to 99.999%; And / or, the particle size D50 of the alumina powder is 0.5 μm to 1.0 μm.

9. The powder coating and sintering method of a ceramic substrate according to claim 7, characterized in that: In the step of preparing the slurry, alumina powder, a dispersant and a sintering aid are mixed in an organic solvent.

10. A ceramic substrate prepared by the powder coating and sintering method of any one of claims 1 to 9.

Citation Information

Patent Citations

  • Powder laying technology and system for ceramic substrate blank body

    CN108058264A

  • Batch sintering method of high-performance silicon nitride ceramic substrate

    CN112811912A

  • High-purity ultrathin high-strength aluminum oxide ceramic substrate as well as preparation method and application thereof

    CN114538900A

Cited By

  • Method for improving flatness of DCB ceramic chip and reducing DCB sintering bubbles

    CN121929997A