Aerogel atomizing core and preparation method thereof
By preparing the aerogel atomized core, porous silicon carbide fibers are generated by chemical reactions between carbon sources and silicon sources, and through chemical vapor permeation strengthening treatment, the existing atomized core strength and oil absorption performance are solved, achieving high The balance of strength and excellent oil absorption performance improves the safety and user experience of e-cigarettes.
Patent Information
- Application Number
- CN202411193349.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-22
AI Technical Summary
Existing electronic cigarette atomized cores such as cotton cores and ceramic cores increase porosity and pore size to pursue taste, resulting in reduced strength and powder loss problems, and poor oil absorption performance.
Using the preparation method of aerogel atomized core, the press molding of mixed carbon source, the first silicon source and the binder is sintered to form a porous silicon carbide fiber aerogel blank, and strengthened by chemical vapor-phase penetration method to form Heat the layer to improve the strength and oil absorption performance of the overall structure.
The high strength and excellent oil absorption performance of the aerogel atomization core are achieved, avoiding powder loss and improving safety performance while maintaining a good atomization experience.
Smart Images

Figure CN118993757A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electronic cigarette atomization, and in particular to an aerogel atomization core and a preparation method thereof. Background Art
[0002] With the development of science and technology, e-cigarettes, as a new type of smoking method, are becoming more and more popular among consumers because of their less harm to health. The core component of e-cigarettes is the atomizer core, whose main function is to heat the e-liquid into atomizers to produce smoke for users to inhale. At present, the commonly used atomizer cores on the market are mainly cotton cores and ceramic cores. As the first generation of atomizer cores, cotton cores are deeply loved by smokers because of their large pore size and large amount of smoke after atomization, but they have problems such as high oil permeability, easy oil leakage, and low taste consistency; the second generation of ceramic cores solves the above problems to a certain extent, but also creates new problems. For example, in order to pursue a taste similar to that of cotton cores, the porosity and pore size are increased, and the oil conduction performance is improved, but it also leads to a decrease in strength and obvious powder loss problems. Summary of the invention
[0003] Based on this, the first aspect of the present application provides a method for preparing an aerogel atomization core, and its technical solution is as follows:
[0004] A method for preparing an aerogel atomization core comprises the following steps:
[0005] mixing a carbon source, a first silicon source and a binder, and pressing the obtained mixture into a shape to obtain a green body;
[0006] Sintering the green body to obtain a porous silicon carbide fiber aerogel body;
[0007] Using the second silicon source as the main reaction source, the porous silicon carbide fiber aerogel blank is strengthened by a chemical vapor infiltration method to obtain a porous inorganic fiber aerogel;
[0008] A heating layer is formed on the porous inorganic fiber aerogel to obtain an aerogel atomization core.
[0009] In one embodiment, the carbon source comprises carbon fiber. Optionally, the carbon fiber comprises graphite fiber.
[0010] In one embodiment, the first silicon source and the second silicon source each independently include a substance that can be decomposed into a silicon-containing gas.
[0011] In one embodiment, the first silicon source and the second silicon source each independently include at least one of silicon monoxide, silicon dioxide, silicon powder, siloxane, dimethyldimethoxysilane, trichloromethylsilane, trimethylchlorosilane and hexamethyldisilazane.
[0012] In one embodiment, the binder is selected from at least one of cellulose, starch, polyacrylic acid, carrageenan, gelatin and water.
[0013] In one embodiment, the chemical vapor infiltration conditions include: the flow rate of the second silicon source is 0.005 g / min to 500 g / min.
[0014] In one embodiment, the chemical vapor infiltration conditions include: introducing a gas, the flow rate of the gas is 0.05 mL / min to 500 mL / min, and the gas is a mixture of hydrogen and argon.
[0015] In one embodiment, the chemical vapor infiltration conditions include: heating at a rate of 1°C / min to 100°C / min to a temperature of 800°C to 1500°C.
[0016] In one embodiment, the sintering conditions include: heating at a rate of 2°C / min to 20°C / min to a temperature of 1300°C to 1800°C.
[0017] In one embodiment, the sintering conditions include: the insulation time is 0.5h~24h.
[0018] In one embodiment, the pressing pressure is 1 MPa~20 MPa.
[0019] In one of the embodiments, the heating layer is formed by printing a resistor paste, sputtering a resistor layer, or laminating a heating mesh.
[0020] A second aspect of the present application provides an aerogel atomization core, which is prepared by the preparation method as described above.
[0021] Compared with the traditional solution, this application has the following beneficial effects:
[0022] The present application utilizes a binder and compression molding to press a carbon source and a first silicon source into a green body, and then through sintering, the carbon source and the first silicon source react to generate silicon carbide fibers, thereby obtaining a porous silicon carbide fiber aerogel body. A second silicon source is then used as the main reaction source. During the chemical vapor infiltration process, the reaction gas generated by the second silicon source diffuses into the interior of the porous silicon carbide fiber aerogel body, and a chemical reaction occurs inside to generate a coating, thereby making the internal fiber connections of the porous silicon carbide fiber aerogel body more firmly connected, thereby obtaining a porous inorganic fiber aerogel with a stable overall structure. After a heating layer is formed thereon, the obtained aerogel atomization core has both high strength and excellent oil absorption performance.
[0023] The aerogel atomizer core described in the present application is an emerging atomization technology product and has been successfully applied in the e-cigarette market with its unique internal structure and physical properties. On the one hand, its higher porosity brings good oil absorption performance. On the other hand, its fiber knot improves the overall strength of the atomizer core, thus achieving a balance between oil absorption performance and strength. While maintaining a good atomization experience, foreign matter will not be inhaled due to powder loss, thereby greatly improving safety performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0025] Figure 1 This is a SEM image of the porous inorganic fiber aerogel prepared in Example 1;
[0026] Figure 2 This is a schematic diagram of the structure of the aerogel atomization core prepared in Example 1. DETAILED DESCRIPTION
[0027] The present application will be further described in detail below in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly understood.
[0028] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0029] the term
[0030] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0031] In the present application, "plurality", "multiple", "multiple times", "plurality", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0032] In this application, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0033] In this application, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0034] In the present application, when referring to a numerical interval (i.e., a numerical range), unless otherwise specified, the optional numerical distribution within the above numerical interval is deemed to be continuous and includes the two numerical endpoints of the numerical range (i.e., the minimum value and the maximum value), and every numerical value between the two numerical endpoints.
[0035] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0036] In the present application, the percentage content, unless otherwise specified, refers to mass percentage for solid-liquid mixing and solid-solid mixing, and volume percentage for liquid-liquid mixing.
[0037] In this application, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.
[0038] In the present application, %(w / w) and wt% both refer to weight percentage, %(v / v) refers to volume percentage, and %(w / v) refers to mass volume percentage.
[0039] At present, there are two main types of atomizer cores commonly used on the market: cotton cores and ceramic cores. As the first generation of atomizer cores, cotton cores are deeply loved by smokers because of their large pore size and large amount of smoke after atomization. However, they have problems such as high oil permeability, easy oil leakage, and low taste consistency. The second generation of ceramic cores has solved the above problems to a certain extent, but it has also created new problems. For example, in order to pursue a taste similar to that of cotton cores, the porosity and pore size are increased, and the oil conduction performance is improved, but it also leads to a decrease in strength and obvious powder loss problems.
[0040] In view of this problem, the first aspect of the present application provides a method for preparing an aerogel atomization core. In one embodiment, the method for preparing an aerogel atomization core comprises the following steps:
[0041] S10, mixing a carbon source, a first silicon source and a binder, and pressing the obtained mixture into a shape to obtain a green body.
[0042] Optionally, the carbon source includes carbon fiber. Further optionally, the carbon fiber includes graphite fiber. Graphite fiber is a fiber with a layered hexagonal lattice graphite structure whose molecular structure has been graphitized and whose carbon content is higher than 99%. Optionally, the aspect ratio of the graphite fiber is in the range of (20-50):1.
[0043] Optionally, the first silicon source includes a substance that can be decomposed into a silicon-containing gas. Further optionally, the first silicon source includes a substance that can be decomposed into a silicon-containing gas at or below the subsequent sintering temperature. Further optionally, the first silicon source includes at least one of silicon monoxide, silicon dioxide, silicon powder, siloxane, dimethyldimethoxysilane, trichloromethylsilane, trimethylchlorosilane and hexamethyldisilazane. In one example, the first silicon source can be provided by a silica sol, which includes water and a first silicon source dispersed in water.
[0044] Optionally, the binder is selected from at least one of cellulose, starch, polyacrylic acid, carrageenan, gelatin and water.
[0045] Optionally, the mass ratio of the carbon source, the first silicon source and the binder is 1: (0.05-0.3): (0.7-1.5). For example, the mass ratio of the carbon source, the first silicon source and the binder is 1: 0.05: 0.7, 1: 0.1: 1, 1: 0.3: 1.5. In one example, the mixture of the carbon source, the first silicon source and the binder is semi-solid.
[0046] The mixture can be placed in a hot pressing mold to press the mixture into a shape. The shape of the molding can be designed according to the shape of the aerogel atomization core, for example, designed to be cylindrical or block-shaped. Through compression molding, the carbon source and the first silicon source can be pressed into a green body of a corresponding shape.
[0047] Optionally, the pressure of the press molding is 1 MPa to 20 MPa. It can be understood that the pressure of the press molding includes but is not limited to 1 MPa, 5 MPa, 10 MPa, 15 MPa, and 20 MPa.
[0048] Optionally, the time for compression molding is 1 hour to 3 hours. It can be understood that the time for compression molding includes but is not limited to 1 hour, 2 hours, and 3 hours.
[0049] S20, sintering the green body to obtain a porous silicon carbide fiber aerogel body.
[0050] It can be understood that before sintering the green body, a drying step is also included. After drying, sintering is performed, and through sintering, the carbon source reacts with the first silicon source to generate silicon carbide fibers.
[0051] Optionally, the sintering temperature program includes: heating at a rate of 2°C / min to 20°C / min to a temperature of 1300°C to 1800°C. For example, heating at a rate of 2°C / min, 5°C / min, 10°C / min, 15°C / min, 20°C / min to a temperature of 1300°C, 1500°C, 1700°C, 1800°C.
[0052] Optionally, the sintering holding time is 0.5h~24h. It can be understood that the sintering holding time includes but is not limited to 0.5h, 2h, 5h, 10h, 20h, and 24h.
[0053] Optionally, the sintering temperature reduction program includes a temperature reduction rate of 8°C / min to 12°C / min to a temperature of 10°C to 40°C. For example, the temperature reduction rate is 8°C / min, 10°C / min, 12°C / min to a temperature of 10°C, 20°C, 30°C, 40°C.
[0054] It can be understood that during the sintering process, argon can be used as a protective gas.
[0055] S30, using the second silicon source as a main reaction source, strengthening the porous silicon carbide fiber aerogel blank by chemical vapor infiltration to obtain a porous inorganic fiber aerogel.
[0056] Chemical Vapor Infiltration (CVI) is a technology that decomposes one or more gas compounds through chemical reactions under high temperature conditions, and the generated active substances are deposited inside the porous medium, thereby densifying the material.
[0057] Further optionally, the second silicon source includes a substance that can be decomposed into a silicon-containing gas in a chemical vapor infiltration chamber. Further optionally, the second silicon source includes at least one of silicon monoxide, silicon dioxide, silicon powder, siloxane, dimethyldimethoxysilane, trichloromethylsilane, trimethylchlorosilane and hexamethyldisilazane.
[0058] Optionally, the flow rate of the second silicon source is 0.005 g / min to 500 g / min. For example, the flow rate of the second silicon source is 0.005 g / min, 0.05 g / min, 0.5 g / min, 5 g / min, 50 g / min, or 500 g / min.
[0059] It is understood that during the chemical vapor infiltration process, a gas is introduced, and the gas includes a mixture of hydrogen and argon. Optionally, the gas flow rate is 0.05 mL / min to 500 mL / min. For example, the gas flow rate is 0.05 mL / min, 0.5 mL / min, 5 mL / min, 50 mL / min, and 500 mL / min.
[0060] Optionally, the temperature increase program of the chemical vapor infiltration method includes: increasing the temperature at a rate of 1°C / min to 100°C / min to a temperature of 800°C to 1500°C. For example, increasing the temperature at a rate of 1°C / min, 10°C / min, 50°C / min, 100°C / min to a temperature of 800°C, 1000°C, 1500°C.
[0061] During the chemical vapor infiltration process, the reaction gas generated by the second silicon source diffuses into the interior of the porous silicon carbide fiber aerogel body and undergoes a chemical reaction inside to form a coating, making the internal fiber connections of the porous silicon carbide fiber aerogel body more firmly connected, which is beneficial to improving the strength of the aerogel atomization core.
[0062] S40, forming a heating layer on the porous inorganic fiber aerogel to prepare an aerogel atomization core.
[0063] Optionally, the heating layer is formed by printing a resistor paste, sputtering a resistor layer, or laminating a heating mesh.
[0064] In one example, the method for forming a heating layer on the porous inorganic fiber aerogel comprises the following steps:
[0065] A resistor paste is printed on the porous inorganic fiber aerogel to form the heating layer.
[0066] The above-mentioned embodiment utilizes a binder and compression molding to press the carbon source and the first silicon source into a green body, and then through sintering, the carbon source and the first silicon source react to generate silicon carbide fibers, and a porous silicon carbide fiber aerogel body is obtained. Then, the second silicon source is used as the main reaction source. During the chemical vapor infiltration process, the reaction gas generated by the second silicon source diffuses into the interior of the porous silicon carbide fiber aerogel body, and a chemical reaction occurs inside to generate a coating, so that the internal fiber connection of the porous silicon carbide fiber aerogel body is more firmly established, and a porous inorganic fiber aerogel with a porous surface and a dense interior is obtained. After a heating layer is formed thereon, the obtained aerogel atomization core has both high strength and excellent oil absorption performance, and generates heat evenly during use, and has a good atomization effect.
[0067] In addition, the preparation method of the aerogel atomization core is simple, efficient, low-cost, and conducive to large-scale production.
[0068] A second aspect of the present application provides an aerogel atomization core. In one embodiment, the aerogel atomization core is prepared by the preparation method as described above.
[0069] The aerogel atomizer core described in the present application is an emerging atomization technology product and has been successfully applied in the e-cigarette market with its unique internal structure and physical properties. On the one hand, its higher porosity brings good oil absorption performance. On the other hand, its fiber knot improves the overall strength of the atomizer core, thus achieving a balance between oil absorption performance and strength. While maintaining a good atomization experience, foreign matter will not be inhaled due to powder loss, thereby greatly improving safety performance.
[0070] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.
[0071] Example 1
[0072] This embodiment provides an aerogel atomization core and a preparation method thereof, and the steps are as follows:
[0073] Step 1: Prepare raw materials, including graphite fiber, silica sol, cellulose and water. The purity of graphite fiber is 99.9%, and the aspect ratio is (20-50):1. The silica sol includes silicon dioxide and water, and the solid content is 30%. The purity of cellulose is 99.5%, and the water is deionized water.
[0074] Step 2: Graphite fiber, silica sol, cellulose and water are mixed in a mass ratio of 1:0.5:0.2:1. Mechanical stirring is adopted during the mixing process. The stirring speed is 500 rpm and the stirring time is 30 min to obtain a semi-solid mixture.
[0075] Step 3: Pour the mixture into a hot pressing mold, the shape of the mold is cylindrical, the diameter is 5 mm, and the height is 20 mm. Then put the mold into a hot pressing machine for hot pressing, the hot pressing temperature is 1500°C, the hot pressing pressure is 5 MPa, and the hot pressing time is 2 hours to obtain a green body.
[0076] Step 4: Dry the pressed green body in a drying oven at a drying temperature of 80° C. for 30 minutes to remove moisture.
[0077] Step 5: Place the dried green body into an atmosphere furnace for sintering. During the sintering process, argon is used as a protective gas. The temperature is raised at a rate of 5°C / min. When the temperature reaches 1500°C, it is kept warm for 2 hours. Then, the temperature is rapidly lowered at a rate of 10°C / min to obtain a well-grown porous SiC fiber aerogel body.
[0078] Step 6: Place the porous SiC fiber aerogel blank in a CVD furnace, use trichloromethylsilane as the second silicon source, use the second silicon source as the reaction source, introduce a mixed gas of hydrogen and argon, control the flow rate of the second silicon source to 2g / min, and the gas flow rate to 10mL / min. Raise the temperature of the CVD furnace to 1100°C at a rate of 5°C / min for gas phase infiltration. After 300 minutes, cool down to obtain a porous inorganic fiber aerogel, and its SEM picture is as follows: Figure 1 shown.
[0079] Step 7: The porous inorganic fiber aerogel is in a cylindrical shape, and then the resistor slurry is printed on the surface to form a heating layer to obtain the final aerogel atomization core. The structure is shown in Figure 2 The aerogel atomization core 100 includes a porous inorganic fiber aerogel 11 in a cylindrical shape and a heating layer 12 on the surface.
[0080] Example 2
[0081] This embodiment provides an aerogel atomization core and a preparation method thereof, which is basically the same as that of Embodiment 1, except that in step 6, the flow rate of the second silicon source is controlled differently. The steps are as follows:
[0082] Step 1: Prepare raw materials, including graphite fiber, silica sol, cellulose and water. The purity of graphite fiber is 99.9%, and the aspect ratio is (20-50):1. The silica sol includes silicon dioxide and water, and the solid content is 30%. The purity of cellulose is 99.5%, and the water is deionized water.
[0083] Step 2: Graphite fiber, silica sol, cellulose and water are mixed in a mass ratio of 1:0.5:0.2:1. Mechanical stirring is adopted during the mixing process. The stirring speed is 500 rpm and the stirring time is 30 min to obtain a semi-solid mixture.
[0084] Step 3: Pour the mixture into a hot pressing mold, the shape of the mold is cylindrical, the diameter is 5 mm, and the height is 20 mm. Then put the mold into a hot pressing machine for hot pressing, the hot pressing temperature is 1500°C, the hot pressing pressure is 5 MPa, and the hot pressing time is 2 hours to obtain a green body.
[0085] Step 4: Dry the pressed green body in a drying oven at a drying temperature of 80° C. for 30 minutes to remove moisture.
[0086] Step 5: Place the dried green body into an atmosphere furnace for sintering. Use argon as the protective gas during the sintering process. Raise the temperature at a rate of 5°C / min. Keep the temperature at 1500°C for 2 hours, then cool it down quickly at a rate of 10°C / min to obtain a well-grown porous SiC fiber body.
[0087] Step six: Place the porous SiC fiber blank in a CVD furnace, use trichloromethylsilane as the second silicon source, use the second silicon source as the reaction source, introduce a mixed gas of hydrogen and argon, control the flow rate of the second silicon source to 4g / min, and the gas flow rate to 10mL / min, and heat the CVD furnace to 1100℃ at a rate of 5℃ / min for gas infiltration. After 300 minutes, cool down to obtain a porous inorganic fiber aerogel.
[0088] Step 7: The porous inorganic fiber aerogel is in a cylindrical shape, and then a resistor slurry is printed on the surface to form a heating layer to obtain the final aerogel atomization core.
[0089] Example 3
[0090] This embodiment provides an aerogel atomization core and a preparation method thereof, which is basically the same as that of Embodiment 1, except that the flow rate of the second silicon source is controlled differently in step 6. The steps are as follows:
[0091] Step 1: Prepare raw materials, including graphite fiber, silica sol, cellulose and water. The purity of graphite fiber is 99.9%, and the aspect ratio is (20-50):1. The silica sol includes silicon dioxide and water, and the solid content is 30%. The purity of cellulose is 99.5%, and the water is deionized water.
[0092] Step 2: Graphite fiber, silica sol, cellulose and water are mixed in a mass ratio of 1:0.5:0.2:1. Mechanical stirring is adopted during the mixing process. The stirring speed is 500 rpm and the stirring time is 30 min to obtain a semi-solid mixture.
[0093] Step 3: Pour the mixture into a hot pressing mold, the shape of the mold is cylindrical, the diameter is 5 mm, and the height is 20 mm. Then put the mold into a hot pressing machine for hot pressing, the hot pressing temperature is 1500°C, the hot pressing pressure is 5 MPa, and the hot pressing time is 2 hours to obtain a green body.
[0094] Step 4: Dry the pressed green body in a drying oven at a drying temperature of 80° C. for 30 minutes to remove moisture.
[0095] Step 5: Place the dried green body into an atmosphere furnace for sintering. Use argon as the protective gas during the sintering process. Raise the temperature at a rate of 5°C / min. Keep the temperature at 1500°C for 2 hours, then cool it down quickly at a rate of 10°C / min to obtain a well-grown porous SiC fiber body.
[0096] Step six: Place the porous SiC fiber blank in a CVD furnace, use trichloromethylsilane as the second silicon source, use the second silicon source as the reaction source, introduce a mixed gas of hydrogen and argon, control the flow rate of the second silicon source to 5 g / min, and the gas flow rate to 10 mL / min, and heat the CVD furnace to 1100 °C at a rate of 5 °C / min for gas infiltration. After 300 minutes, cool down to obtain a porous inorganic fiber aerogel.
[0097] Step 7: The porous inorganic fiber aerogel is in a cylindrical shape, and then a resistor slurry is printed on the surface to form a heating layer to obtain the final aerogel atomization core.
[0098] The performance of the above embodiments is tested, and the testing method is as follows:
[0099] Porosity test method: Based on the Archimedes buoyancy principle, a dedicated density and porosity tester is used to test the porosity of the aerogel atomization core.
[0100] Strength test reference standard: The strength of the aerogel atomization core is tested using the national standard "GB / T 4740-1999" method.
[0101] Oil absorption performance test method: Use cigarette oil for internal standard test, test the time taken for the cigarette oil to reach the upper plane from the bottom surface, the test cigarette oil is composed of 50% propylene glycol and 50% glycerol (glycerol), and each embodiment formula is tested with 3 samples, and the average value is the oil absorption rate of the embodiment sample, unit s. This test uses the same atomization medium to test the oil absorption speed, take glycerol (VG) and propylene glycol (PG) mixed solvent and place it in a container, where PG: VG = 1: 1, put a sponge in the container, the height of the sponge is higher than the liquid level, and place the porous substrate parallel to the sponge, start timing until the cigarette oil rises from the bottom surface to the upper plane of the substrate through capillary force.
[0102] The test results are shown in Table 1.
[0103] Table 1
[0104]
[0105] It can be seen that the aerogel atomization core prepared by each embodiment of the present application has both high strength and good oil absorption performance.
[0106] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0107] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A method for preparing an aerogel atomization core, characterized in that: The following steps are involved: mixing a carbon source, a first silicon source and a binder, and pressing the obtained mixture into a shape to obtain a green body; Sintering the green body to obtain a porous silicon carbide fiber aerogel body; Using the second silicon source as the main reaction source, the porous silicon carbide fiber aerogel blank is strengthened by a chemical vapor infiltration method to obtain a porous inorganic fiber aerogel; A heating layer is formed on the porous inorganic fiber aerogel to obtain an aerogel atomization core.
2. The method for preparing the aerogel atomization core according to claim 1, characterized in that: The carbon source includes carbon fibers.
3. The method for preparing the aerogel atomization core according to claim 1, characterized in that: The first silicon source and the second silicon source each independently include a substance that can be decomposed into a silicon-containing gas.
4. The method for preparing the aerogel atomization core according to claim 3, characterized in that: The first silicon source and the second silicon source each independently include at least one of silicon monoxide, silicon dioxide, silicon powder, siloxane, dimethyldimethoxysilane, trichloromethylsilane, trimethylchlorosilane and hexamethyldisilazane.
5. The method for preparing an aerogel atomization core according to claim 1, characterized in that: The binder is selected from at least one of cellulose, starch, polyacrylic acid, carrageenan, gelatin and water.
6. The method for preparing an aerogel atomization core according to any one of claims 1 to 5, characterized in that: The chemical vapor infiltration conditions include at least one of the following conditions: (1) The flow rate of the second silicon source is 0.005 g / min to 500 g / min; (2) introducing gas at a flow rate of 0.05 mL / min to 500 mL / min, wherein the gas is a mixture of hydrogen and argon; (3) Heating at a rate of 1°C / min to 100°C / min to a temperature of 800°C to 1500°C.
7. The method for preparing an aerogel atomization core according to any one of claims 1 to 5, characterized in that: The sintering conditions include at least one of the following conditions: (1) Heating at a rate of 2°C / min~20°C / min to a temperature of 1300°C~1800°C; (2) The insulation time is 0.5h~24h.
8. The method for preparing an aerogel atomization core according to any one of claims 1 to 5, characterized in that: The pressure of the pressing molding is 1MPa~20MPa.
9. The method for preparing an aerogel atomization core according to any one of claims 1 to 5, characterized in that: The heating layer is formed by printing a resistor paste, sputtering a resistor layer, or laminating a heating mesh.
10. An aerogel atomization core, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of micro-nanofiber / ceramic matrix composite
CN104803685A
Aerogel material composed of fibers and adhesive, and preparation method and application thereof
CN107868270A
High-temperature-resistant light-weight high-strength porous ceramic and preparation method thereof
CN114276163A
Silicon carbide aerogel and preparation method thereof
CN114716229A
Lightweight high-strength porous ceramic with electromagnetic shielding effectiveness and preparation method and application thereof
CN116444293A