Macromolecular alpha-diimine nickel and palladium catalyst as well as preparation method and application thereof

CN118994484AActive Publication Date: 2024-11-22CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411077533.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

然而,虽然通过调控配体的空间效应与电子效应,可以得到高支化聚合物,但是聚合活性却普遍不高,难以高效制备聚烯烃弹性体

Benefits of technology

[0045] Based on the norbornenedione and cyclooctenedione skeletons containing cyclic double bonds, the present invention develops a new type of macromolecular α-diimide nickel and palladium catalysts. Through ring-opening ectopic polymerization, single-core The catalyst can be easily converted into a macromolecular multi-nuclear catalyst, which avoids the side reaction of bimolecular deactivation in a small molecule catalytic system and improves its catalytic activity and thermal stability in ethylene polymerization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004982777030000021
    Figure BDA0004982777030000021
  • Figure BDA0004982777030000031
    Figure BDA0004982777030000031
  • Figure BDA0004982777030000032
    Figure BDA0004982777030000032
Patent Text Reader

Abstract

The invention provides a macromolecular alpha-diimine nickel and palladium catalyst as well as a preparation method and application thereof. The macromolecular alpha-diimine nickel and palladium catalyst provided by the invention has a structure as shown in a formula I or II, a skeleton contains double bonds, the structure is special, and when the macromolecular alpha-diimine nickel and palladium catalyst is used as a catalyst for catalyzing ethylene polymerization, the catalytic activity is high and can reach 2.5 * 107 g mol <-1 > h <-1 > or above; the molecular weight and the branching degree of the prepared polymer are greatly adjustable, and branched polyolefin with the molecular weight of 0.3-38.0 million and the branching degree of 48-111 / 1000C can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of olefin catalysis, and specifically relates to a macromolecular α-diimine nickel and palladium catalyst, and a preparation method and application thereof. Background Art

[0002] Since 1995, due to the unique chain walking mechanism, α-diimine post-transition metal nickel and palladium catalysts have received widespread attention from academia and industry. A document (J.Am.Chem.Soc.1995,117,6414) reported that α-diimine nickel and palladium catalysts have now become a very useful class of ethylene polymerization catalysts, which can be used to prepare branched polyolefins with ethylene as the only monomer. However, the document (Eur.Polym.J.2022,181,111693) pointed out that there are still some unresolved problems in this catalytic system, such as the catalyst is not active enough under high temperature conditions and cannot be applied to industrial production.

[0003] In order to solve this kind of problem, the commonly used method is to modify the catalyst ligand structure and adjust the electronic effect and steric effect of the ligand to improve the thermal stability of the catalyst. However, although highly branched polymers can be obtained by regulating the spatial effect and electronic effect of the ligand, the polymerization activity is generally not high, and it is difficult to prepare polyolefin elastomers efficiently. In addition, the catalyst has poor heat resistance, especially at temperatures above 70°C, with low molecular weight and low activity. These two points limit the application of α-diimine nickel and palladium catalysts to a certain extent. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a macromolecular α-diimine nickel and palladium catalyst, and a preparation method and application thereof. The catalyst has high catalytic activity, and the molecular weight and branching degree of the prepared polymer can be greatly adjusted.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In the first aspect, the present invention provides a macromolecular α-diimine nickel and palladium catalyst having a structure shown in Formula I or II:

[0007]

[0008] Among them, R 1 , R 2 , R 4 and R 5 Each is independently selected from substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C6-C30 aryl;

[0009] R 3 and R 6Each is independently selected from hydrogen, hydroxy, halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C1-C6 alkoxy;

[0010] M is nickel or palladium;

[0011] X is halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C6-C30 aryl;

[0012] The value of n is 2 to 1000.

[0013] Preferably, the R 1 , R 2 , R 4 and R 5 Each is independently selected from a substituted or unsubstituted C1-C4 alkyl group and a substituted or unsubstituted C6-C20 aryl group.

[0014] Preferably, R 3 and R 6 Each is independently selected from hydrogen, hydroxy, halogen, substituted or unsubstituted C1-C4 alkyl, and substituted or unsubstituted C1-C4 alkoxy.

[0015] Preferably, X is halogen, substituted or unsubstituted C1-C4 alkyl, or substituted or unsubstituted C6-C20 aryl.

[0016] More preferably, the R 1 , R 2 , R 4 and R 5 Each is independently selected from methyl, phenyl, isopropyl or benzhydryl.

[0017] More preferably, R 3 and R 6 Each is independently selected from hydrogen, methyl, hydroxy, halogen or methoxy.

[0018] More preferably, X is halogen, substituted or unsubstituted C1-C3 alkyl, or substituted or unsubstituted C6-C18 aryl.

[0019] Further preferably, the macromolecular α-diimine nickel and palladium catalyst is selected from any one of formulas Ⅰ-1 to Ⅰ-10 or formulas Ⅱ-1 to Ⅱ-10:

[0020]

[0021] In a second aspect, the present invention also provides a method for preparing the above-mentioned macromolecular α-diimine nickel and palladium catalyst having a structure shown in formula I or formula II, comprising:

[0022] S1-1: mixing norbornene dione or cyclooctenedione with a substituted aromatic amine represented by formula A and reacting them to obtain a compound represented by formula L1 or formula L2;

[0023] S2-1: mixing and reacting the compound represented by formula L1 or formula L2 with a nickel source or a palladium source to obtain a compound represented by formula C1 or formula C2;

[0024] S3-1: polymerizing the compound represented by formula C1 or formula C2 in the presence of a catalyst to obtain a macromolecular α-diimine nickel or palladium catalyst represented by formula I or formula Ⅰ;

[0025]

[0026] or

[0027] S1-2: According to the method of S1-1, a compound represented by formula L1 or formula L2 is obtained;

[0028] S2-2: polymerizing the compound represented by formula L1 or formula L2 in the presence of a catalyst to obtain a compound represented by formula L1-P or L2-P;

[0029] S3-2: mixing and reacting the compound represented by formula L1-P or L2-P with a nickel source or a palladium source to obtain a macromolecular α-diimine nickel and palladium catalyst represented by formula I or formula Ⅰ;

[0030]

[0031] Preferably, the molar ratio of the norbornene dione or cyclooctenedione to the substituted aromatic amine represented by formula A is 1:1 to 1:20.

[0032] Preferably, the molar ratio of the compound represented by Formula L1 or Formula L2 to the nickel source or palladium source is 1:1 to 1:10.

[0033] Preferably, the molar ratio of the compound represented by Formula C1 or Formula C2 to the catalyst is 10:1 to 1000:1.

[0034] Preferably, the molar ratio of the compound represented by Formula L1 or Formula L2 to the catalyst is 10:1 to 1000:1.

[0035] Preferably, the molar ratio of the compound represented by formula L1-P or formula L2-P to the nickel source or palladium source is 1:n.

[0036] Preferably, the reaction temperature in step S1-1 is 20 to 80° C., and the reaction time is 2 to 10 h.

[0037] Preferably, the reaction temperature in step S2-1 or step S3-2 is independently 15 to 30° C., and the reaction time is independently 40 to 90 h.

[0038] Preferably, the polymerization temperature in step S2-2 or step S3-1 is independently 15 to 30° C., and the polymerization time is independently 5 to 20 hours.

[0039] Preferably, the nickel source is selected from ethylene glycol dimethyl ether nickel bromide and / or ethylene glycol dimethyl ether nickel chloride.

[0040] Preferably, the palladium source is selected from chloro(1,5-cyclooctadiene)methylpalladium(II).

[0041] Preferably, the catalyst is selected from any one or more of a Grubbs I catalyst, a Grubbs II catalyst, a Grubbs III catalyst, a Hoveyda-Grubbs I catalyst or a Hoveyda-Grubbs II catalyst.

[0042] In a third aspect, the present invention provides an application of the above-mentioned macromolecular α-diimine nickel and palladium catalyst in ethylene polymerization.

[0043] Preferably, in the above application, the application temperature of the macromolecular α-diimine nickel and palladium catalyst is ≥ 0°C.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] The present invention develops a new type of macromolecular α-diimine nickel and palladium catalysts based on norbornene dione and cyclooctenedione skeletons containing cyclic double bonds. Through ring-opening heterotopic polymerization, the mononuclear catalyst can be simply converted into a macromolecular multinuclear catalyst, avoiding the side reaction of bimolecular deactivation in the small molecule catalytic system, and improving its catalytic activity and thermal stability in ethylene polymerization.

[0046] According to the test, the catalytic activity of the macromolecular α-diimine nickel and palladium catalyst provided by the present invention is high, which can reach 2.5×10 7 g mol -1 h -1 The above; and the molecular weight and branching degree of the polymer prepared by using it as a catalyst for catalyzing ethylene polymerization can be greatly adjusted, and branched polyolefins with a molecular weight of 0.3 to 380,000 and a branching degree of 48-111 / 1000C can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 is the single crystal diffraction pattern of the α-diimine nickel complex Ni3 in Example 7;

[0048] Figure 2 is the hydrogen spectrum of the prepared polymer corresponding to No. 11 in Table 3;

[0049] Figure 3 The stress-strain curves of the prepared polymers corresponding to Nos. 5, 9, and 10 in Table 3;

[0050] Figure 4 This is the elastic recovery curve of the polymer prepared corresponding to No. 5 in Table 3. DETAILED DESCRIPTION

[0051] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0052] At present, although α-diimine nickel and palladium catalysts can obtain highly branched polymers by regulating the spatial effect and electronic effect of the ligand in catalyzing ethylene polymerization, the polymerization activity is generally not high, making it difficult to efficiently prepare polyolefin elastomers. In addition, α-diimine nickel and palladium catalysts have poor heat resistance, especially at temperatures above 70°C, and have low molecular weight and activity. These two points limit the application of α-diimine nickel and palladium catalysts to a certain extent.

[0053] Based on this, the present invention innovatively proposes the concept of "macromolecular catalyst" and develops a new type of macromolecular α-diimine nickel and palladium catalysts based on the norbornene dione and cyclooctenedione skeletons containing cyclic double bonds. Through ring-opening heterotopic polymerization, the mononuclear catalyst can be simply converted into a macromolecular multi-nuclear catalyst, thereby improving its catalytic activity and thermal stability in ethylene polymerization.

[0054] In the present invention, the macromolecular α-diimine nickel and palladium catalyst has a structure shown in Formula I or II:

[0055]

[0056] Among them, R 1 , R 2 , R 4 and R 5 Each is independently selected from substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C6-C30 aryl;

[0057] R 3 and R 6 Each is independently selected from hydrogen, hydroxy, halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C1-C6 alkoxy;

[0058] M is nickel or palladium;

[0059] X is halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C6-C30 aryl;

[0060] The value of n is 2 to 1000, and specifically can be 2, 10, 50, 100, 200, 300, 400, 500, 600, 700, 800, 900 or 1000, etc.

[0061] The above point values ​​are only for enumeration. The specific value of n is not limited to this. Other point values ​​within the numerical range are applicable. To avoid complexity, they will not be described one by one.

[0062] In some embodiments of the present invention, the macromolecular α-diimine nickel and palladium catalyst has a structure shown in Formula I or II. 1 , R 2 , R 4 and R 5 Each is independently preferably selected from a substituted or unsubstituted C1-C4 alkyl group, a substituted or unsubstituted C6-C20 aryl group; R 3 and R 6 Each is independently preferably selected from hydrogen, hydroxyl, halogen, substituted or unsubstituted C1-C4 alkyl, substituted or unsubstituted C1-C4 alkoxy; X is preferably halogen, substituted or unsubstituted C1-C4 alkyl, substituted or unsubstituted C6-C20 aryl.

[0063] In other embodiments of the present invention, the macromolecular α-diimine nickel and palladium catalyst has a structure shown in Formula I or II. 1 , R 2 , R 4 and R 5 Each is independently selected from methyl, phenyl, isopropyl or diphenylmethyl; R 3 and R 6 Each is independently selected from hydrogen, methyl, hydroxyl, halogen or methoxy; X is more preferably halogen, substituted or unsubstituted C1-C3 alkyl, substituted or unsubstituted C6-C18 aryl.

[0064] In the present invention, in the above-mentioned "substituted or unsubstituted", the "substituted" group can be selected from C1-C3 alkyl groups or C6-C18 aryl groups.

[0065] In some specific embodiments of the present invention, the macromolecular α-diimine nickel and palladium catalyst is selected from any one of formulas Ⅰ-1 to Ⅰ-10 or formulas Ⅱ-1 to Ⅱ-10:

[0066]

[0067] It should be noted that in the present invention, R 1 , R 2 , R 3 , R 4 and R 5 and R 6 The groups connected to the benzene ring can be the same or different groups.

[0068] The present invention also provides a method for preparing the above macromolecular α-diimine nickel and palladium catalyst. In the present invention, the method for preparing the macromolecular α-diimine nickel and palladium catalyst having the structure shown in formula I has two synthetic routes: route 1 and route 2.

[0069] Among them, route 1 mainly includes the following steps:

[0070] S1-1: mixing norbornene dione with a substituted aromatic amine represented by formula A and reacting them to obtain a compound represented by formula L1;

[0071] S2-1: mixing and reacting the compound represented by formula L1 with a nickel source or a palladium source to obtain a compound represented by formula C1;

[0072] S3-1: polymerizing the compound represented by formula C1 in the presence of a catalyst to obtain a macromolecular α-diimine nickel and palladium catalyst having a structure represented by formula I;

[0073]

[0074] In the present invention, firstly, norbornene dione is mixed with the substituted aromatic amine shown in formula A and reacted to obtain the compound shown in formula L1. Wherein, the molar ratio of the norbornene dione to the substituted aromatic amine shown in formula A is 1:1 to 1:20, preferably 1:2 to 1:5, and more preferably 1:2. The temperature of the reaction is 20 to 80°C, preferably 30 to 60°C, and the reaction time is 2 to 10 hours, preferably 3 to 8 hours. In some embodiments of the present invention, it is preferred to add 1 equivalent of norbornene dione and N equivalents of substituted aromatic amine in a ratio of 1:N (N≥2, the larger N, the shorter the reaction time), and react in a mixed solution of methanol and formic acid at 20 to 80°C for more than 6 hours to obtain the compound shown in formula L1. In some preferred embodiments of the present invention, after the reaction is completed, post-treatment is preferably performed, that is, the reaction solution is cooled (-78°C to 0°C) to precipitate the product, the solid is separated by filtration, washed three times with cold methanol (or cold ethanol) and dried under vacuum conditions to obtain the compound represented by formula L1 (also called "α-diimine ligand"), and the yield is above 10%.

[0075] Then, the compound represented by formula L1 is mixed with a nickel source or a palladium source and reacted to obtain a compound represented by formula C1. In the present invention, the molar ratio of the compound represented by formula L1 to the nickel source or palladium source is 1:1 to 1:10, preferably 1:1 to 1:5, and more preferably 1:1 to 1:2; the nickel source is selected from ethylene glycol dimethyl ether nickel bromide; the palladium source is selected from chloro(1,5-cyclooctadiene)methylpalladium(II). The reaction temperature is 15 to 30°C, preferably 20 to 25°C; the reaction time is 40 to 90h, preferably 48 to 72h. In some embodiments of the present invention, 1 equivalent of α-diimine ligand (formula L1) and 1 equivalent of nickel source or palladium source are added, and stirred at 25°C for 72 hours in a mixed solution of dichloromethane. After the reaction is completed, filter and drain the solvent to obtain the compound represented by formula C1 with a yield of more than 90%.

[0076] Then, according to the present invention, the compound represented by formula C1 is polymerized in the presence of a catalyst to obtain a macromolecular α-diimine nickel and palladium catalyst having a structure represented by formula I. The catalyst is used to catalyze the polymerization of the compound represented by formula C1 itself, and can be specifically selected from Grubbs II catalyst. The polymerization temperature is 15 to 30°C, preferably 20 to 25°C; the reaction time is 5 to 20 hours, preferably 6 to 12 hours. In some embodiments of the present invention, the compound represented by formula C1 is dissolved in dichloromethane to prepare a 0.01 to 0.1M solution, a catalytic amount of Grubbs II catalyst is added, and the mixture is stirred at room temperature for 12 hours. After the reaction is completed, the solution is poured into 40 mL of hexane, filtered and dried to obtain a macromolecular α-diimine nickel and palladium catalyst represented by formula I, with a yield of more than 95%.

[0077] Among them, route 2 of the present invention for synthesizing the macromolecular α-diimine nickel and palladium catalyst shown in formula I mainly comprises the following steps:

[0078] S1-2: mixing norbornene dione with a substituted aromatic amine represented by formula A and reacting them to obtain an α-diimine ligand represented by formula L1;

[0079] S2-2: polymerizing the compound represented by formula L1 in the presence of a catalyst to obtain a compound represented by formula L1-P;

[0080] S3-2: mixing and reacting the compound represented by formula L1-P with a nickel source or a palladium source to obtain a macromolecular α-diimine nickel and palladium catalyst represented by formula I;

[0081]

[0082] In the present invention, the scheme for obtaining the compound represented by formula L1 is as described in the relevant content of the above-mentioned route 1, which will not be repeated here.

[0083] According to the present invention, after obtaining the compound represented by formula L1 in route 2, it is first polymerized in the presence of a catalyst to obtain a compound represented by formula L1-P. The molar ratio of the compound represented by formula L1 to the catalyst is 10:1 to 1000:1, preferably 20:1 to 800:1, and more preferably 50:1 to 300:1. The catalyst is used to catalyze the polymerization of the compound represented by formula L1 itself, and can be specifically selected from Grubbs II catalyst. The polymerization temperature is 15 to 30°C, preferably 20 to 25°C; the reaction time is 5 to 20h, preferably 6 to 12h. In some embodiments of the present invention, the α-diimine ligand (formula L1) is preferably dissolved in dichloromethane to prepare a 0.01 to 0.1M solution, a catalytic amount of Grubbs II catalyst is added, and the mixture is stirred at room temperature for 6 hours. After the reaction is completed, the solution is poured into 40mL of hexane, filtered and dried to obtain L1-P, with a yield of more than 95%.

[0084] Then, the compound represented by formula L1-P is mixed with a nickel source or a palladium source and reacted to obtain a macromolecular α-diimine nickel and palladium catalyst represented by formula I. The molar ratio of the compound represented by formula L1-P to the nickel source or palladium source is 1:n. The selection of the nickel source or palladium source is as described in the relevant content of the above technical scheme, and will not be repeated here. The reaction temperature is 15 to 30°C, preferably 20 to 25°C; the reaction time is 40 to 90h, preferably 48 to 72h. In some embodiments of the present invention, 1 equivalent of the compound represented by formula L1-P and 1 equivalent of the nickel source or palladium source (relative to the polymerization unit in L1-P) are added and stirred at 25°C for 72 hours in a mixed solution of dichloromethane. After the reaction is completed, filter and drain the solvent to obtain the macromolecular α-diimine nickel and palladium catalyst represented by formula I.

[0085] The present invention also provides a method for preparing a macromolecular α-diimine nickel and palladium catalyst having a structure shown in formula II, which also includes two routes, route 1 and route 2.

[0086] Among them, Route 1 mainly includes:

[0087] S1-1: mixing cyclooctenedione with a substituted aromatic amine represented by formula A and reacting them to obtain a compound represented by formula L2;

[0088] S2-1: mixing and reacting the compound represented by formula L2 with a nickel source or a palladium source to obtain a compound represented by formula C2;

[0089] S3-1: polymerizing the compound represented by formula C2 under the action of a catalyst to obtain a macromolecular α-diimine nickel and palladium catalyst having a structure represented by formula ⅠⅠ;

[0090]

[0091] In the present invention, cyclooctenedione is first mixed with a substituted aromatic amine shown in formula A and reacted to obtain a compound shown in formula L2. Wherein, the molar ratio of the cyclooctenedione to the substituted aromatic amine shown in formula A is 1:1 to 1:20, preferably 1:2 to 1:5, and more preferably 1:2. The reaction temperature is 20 to 80°C, preferably 30 to 60°C, and the reaction time is 2 to 10h, preferably 3 to 8h. In some embodiments of the present invention, it is preferred to add 1 equivalent of cyclooctenedione and N equivalents of substituted aromatic amine in a ratio of 1:N (N≥2, the larger the N, the shorter the reaction time), and react in a mixed solution of methanol and formic acid at 20 to 80°C for more than 6 hours to obtain a compound shown in formula L2. In some preferred embodiments of the present invention, after the reaction is completed, post-treatment is preferably performed, that is, the reaction solution is cooled (-78°C to 0°C) to precipitate the product, the solid is separated by filtration, washed three times with cold methanol (or cold ethanol) and dried under vacuum conditions to obtain the compound represented by formula L2, with a yield of more than 10%.

[0092] Then, the compound represented by formula L2 is mixed with a nickel source or a palladium source and reacted to obtain a compound represented by formula C2. In the present invention, the molar ratio of the compound represented by formula L2 to the nickel source or palladium source is 1:1 to 1:10, preferably 1:1 to 1:5, and more preferably 1:1 to 1:2. The nickel source is selected from ethylene glycol dimethyl ether nickel bromide and / or ethylene glycol dimethyl ether nickel chloride; the palladium source is selected from chloro(1,5-cyclooctadiene)methylpalladium(II). The reaction temperature is 15 to 30°C, preferably 20 to 25°C; the reaction time is 40 to 90h, preferably 48 to 72h. In some embodiments of the present invention, 1 equivalent of the compound represented by formula L2 and 1 equivalent of the nickel source or palladium source are added and stirred at 25°C for 72 hours in a mixed solution of dichloromethane. After the reaction is completed, filter and drain the solvent to obtain the compound represented by formula C2 with a yield of more than 90%.

[0093] Then, according to the present invention, the compound shown in formula C2 is polymerized under the action of a catalyst to obtain a macromolecular α-diimine nickel and palladium catalyst having a structure shown in formula I. The catalyst is used to catalyze the polymerization of the compound shown in formula C1 itself, and can be specifically selected from any one or more of Grubbs I catalyst, Grubbs II catalyst, Grubbs III catalyst, Hoveyda-Grubbs I catalyst or Hoveyda-Grubbs II catalyst. The polymerization temperature is 15 to 30°C, preferably 20 to 25°C; the reaction time is 5 to 20h, preferably 6 to 12h. In some embodiments of the present invention, the compound shown in formula C2 is dissolved in dichloromethane to prepare a 0.01 to 0.1M solution, a catalytic amount of Grubbs II catalyst is added, and the mixture is stirred at room temperature for 12 hours. After the reaction is completed, the solution is poured into 40mL of hexane, filtered and dried to obtain a macromolecular α-diimine nickel and palladium catalyst having a structure shown in formula ⅠⅠ, with a yield of more than 95%.

[0094] In the present invention, route 2 of the present invention for synthesizing the macromolecular α-diimine nickel and palladium catalyst shown in formula ⅠⅠ mainly comprises the following steps:

[0095] S1-2: mixing cyclooctenedione with a substituted aromatic amine represented by formula A and reacting them to obtain an α-diimine ligand represented by formula L2;

[0096] S2-2: polymerizing the compound represented by formula L2 under the action of a catalyst to obtain a compound represented by formula L2-P;

[0097] S3-2: mixing and reacting the compound represented by formula L2-P with a nickel source or a palladium source to obtain a macromolecular α-diimine nickel and palladium catalyst represented by formula II;

[0098]

[0099] In the present invention, the scheme for obtaining the compound represented by formula L2 is as described in the relevant content of the above-mentioned route 1, which will not be repeated here.

[0100] According to the present invention, after obtaining the compound represented by formula L1 in route 2, the compound represented by formula L2 is first polymerized under the action of a catalyst to obtain a compound represented by formula L2-P. The molar ratio of the compound represented by formula L2 to the catalyst is 10:1 to 1000:1, preferably 20:1 to 800:1, and more preferably 50:1 to 300:1. The catalyst is used to catalyze the polymerization of the compound represented by formula L2 itself, and can be specifically selected from any one or more of Grubbs I catalyst, Grubbs II catalyst, Grubbs III catalyst, Hoveyda-Grubbs I catalyst or Hoveyda-Grubbs II catalyst. The polymerization temperature is 15 to 30°C, preferably 20 to 25°C; the reaction time is 5 to 20h, preferably 6 to 12h. In some embodiments of the present invention, the compound represented by formula L2 is preferably dissolved in dichloromethane to prepare a 0.01 to 0.1M solution, a catalytic amount of Grubbs II catalyst is added, and the mixture is stirred at room temperature for 6 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a compound represented by formula L2-P with a yield of more than 95%.

[0101] Then, the compound represented by formula L2-P is mixed with a nickel source or a palladium source and reacted to obtain a macromolecular α-diimine nickel and palladium catalyst represented by formula II. The molar ratio of the compound represented by formula L2-P to the nickel source or palladium source is 1:n. The selection of the nickel source or palladium source is as described in the relevant content of the above technical scheme, which will not be repeated here. The temperature of the reaction is 15 to 30°C, preferably 20 to 25°C; the reaction time is 40 to 90h, preferably 48 to 72h. In some embodiments of the present invention, it is preferred to feed according to formula L2-P1 equivalent, nickel source or palladium source 1 equivalent (relative to the polymerization unit in L2-P), and stir in a mixed solution of dichloromethane at 25°C for 72 hours. After the reaction is completed, filter and drain the solvent to obtain a macromolecular α-diimine nickel and palladium catalyst represented by formula ⅠⅠ, with a yield of more than 90%.

[0102] In the present invention, the synthesis route of the macromolecular α-diimine nickel and palladium catalyst represented by the above formula I or II is as follows:

[0103]

[0104] In some embodiments of the present invention, α-diimine nickel catalyst monomers and macromolecular α-diimine nickel catalysts with different polymerization degrees are used as catalysts for ethylene polymerization. It is found that as the polymerization degree of the macromolecular α-diimine nickel catalyst increases, the activity of catalyzing ethylene homopolymerization increases significantly, and the molecular weight increases significantly; and the polymerization reaction of the same catalyst decreases in activity and molecular weight as the temperature increases, and the degree of branching increases. The α-diimine nickel catalyst monomer loses its activity at 90°C, but the macromolecular nickel catalyst still has a high activity at 90°C.

[0105] Similarly, in other embodiments of the present invention, α-diimine palladium catalyst monomers and macromolecular α-diimine palladium catalysts with different polymerization degrees are used as catalysts for ethylene polymerization, and it is found that under the same conditions, the macromolecular α-diimine palladium catalyst has higher polymerization activity than the α-diimine palladium catalyst monomer, and the prepared polymer has a higher molecular weight, a lower degree of branching, and a narrower molecular weight distribution.

[0106] In addition, in some embodiments of the present invention, the α-diimine nickel catalyst monomer and the macromolecular α-diimine nickel catalyst shown in Formula I were also subjected to scale-up experiments. The results showed that under scale-up conditions, the macromolecular α-diimine nickel catalyst can still be used to prepare highly branched polyethylene elastomers with high activity, and the highest activity is 12×10 6 g mol -1 h -1 , i.e. 18kg PE / g Cat In contrast, the α-diimine nickel catalyst monomer has lower activity and molecular weight.

[0107] In summary, the macromolecular α-diimine nickel and palladium catalysts shown in formula I or II provided by the present invention have high catalytic activity, and the molecular weight and branching degree of the prepared polymer can be greatly adjusted. Based on this, the present invention also provides an application of the above macromolecular α-diimine nickel and palladium catalysts in ethylene polymerization.

[0108] In order to further illustrate the present invention, the following examples are provided for detailed description. The experimental raw materials used in the following examples of the present invention are all common commercially available products.

[0109] Example 1

[0110] This embodiment provides an α-diimine ligand L1-1, wherein R1, R2, R4 and R5 are methyl groups, and R3 and R6 are hydrogen;

[0111]

[0112] Norbornene-4,5-dione (0.2853 g, 2.336 mmol) and 2,6-dimethylaniline (0.5662 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. The volatiles were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.5100 g, 60% yield). Example 2

[0113] This embodiment provides an α-diimine nickel complex Ni1, R1, R2, R4 and R5 are methyl groups, R3 and R6 are hydrogen, and X is bromine;

[0114]

[0115] A mixture of α-diimine ligand L1-1 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni1. (0.24 g, 90% yield).

[0116] Example 3

[0117] This embodiment provides an α-diimine nickel complex Ni2, R1, R2, R4 and R5 are methyl, R3 and R6 are hydrogen; X is bromine;

[0118]

[0119] A mixture of catalyst Ni1 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni2. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 9.

[0120] Example 4

[0121] This embodiment provides an α-diimine palladium complex Pd1, R1, R2, R4 and R5 are methyl groups, and R3 and R6 are hydrogen;

[0122]

[0123] A mixture of α-diimine ligand L1-1 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd1 (0.24 g, 90% yield).

[0124] Example 5

[0125] This embodiment provides an α-diimine palladium complex Pd2, R1, R2, R4 and R5 are methyl, R3 and R6 are hydrogen;

[0126]

[0127] A mixture of catalyst Pd1 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd2. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 39.

[0128] Example 6

[0129] This embodiment provides an α-diimine ligand L1-2, wherein R1, R2, R4 and R5 are isopropyl, and R3 and R6 are hydrogen;

[0130]

[0131] The preparation method is as follows:

[0132] Norbornene-4,5-dione (0.2853 g, 2.336 mmol) and 2,6-diisopropylaniline (0.8283 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.1164 g, yield 11%).

[0133] Example 7

[0134] This embodiment provides an α-diimine nickel complex Ni3, R1, R2, R4 and R5 are isopropyl, R3 and R6 are hydrogen; X is bromine;

[0135]

[0136] A mixture of α-diimine ligand L1-2 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni3. (0.24 g, 90% yield).

[0137] The single crystal diffraction pattern of Ni3 is as follows: Figure 1 shown.

[0138] Example 8

[0139] This embodiment provides an α-diimine nickel complex Ni4, R1, R2, R4 and R5 are isopropyl, R3 and R6 are hydrogen; X is bromine;

[0140]

[0141] A mixture of catalyst Ni3 (0.2 g, 0.30 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 5 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 20 mL of hexane, filtered and dried to obtain a brick red solid, namely Ni4. (196 mg, 98% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 5.

[0142] Example 9

[0143] This embodiment provides an α-diimine nickel complex Ni5, R1, R2, R4 and R5 are isopropyl, R3 and R6 are hydrogen; X is bromine;

[0144]

[0145] A mixture of catalyst Ni3 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni5. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 9.

[0146] Example 10

[0147] This embodiment provides an α-diimine palladium complex Pd3, R1, R2, R4 and R5 are isopropyl, R3 and R6 are hydrogen;

[0148]

[0149] A mixture of α-diimine ligand L1-2 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd3 (0.24 g, 90% yield).

[0150] Embodiment 11

[0151] This embodiment provides an α-diimine palladium complex Pd4, R1, R2, R4 and R5 are isopropyl, R3 and R6 are hydrogen;

[0152]

[0153] A mixture of catalyst Pd3 (0.2 g, 0.30 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 5 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 20 mL of hexane, filtered and dried to obtain a brick red solid, namely Pd4. (196 mg, 98% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 11.

[0154] Example 12

[0155] This embodiment provides an α-diimine palladium complex Pd5, R1, R2, R4 and R5 are isopropyl, R3 and R6 are hydrogen;

[0156]

[0157] A mixture of catalyst Pd3 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd5. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 19.

[0158] Example 13

[0159] This embodiment provides an α-diimine ligand L1-3, wherein R1, R2, R4 and R5 are methyl groups, and R3 and R6 are hydroxy groups;

[0160]

[0161] Norbornene-4,5-dione (0.2853 g, 2.336 mmol) and 2,6-dimethyl-4-hydroxy-aniline (0.6317 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. The volatiles were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.5227 g, 57% yield).

[0162] Embodiment 14

[0163] This embodiment provides an α-diimine nickel complex Ni6, wherein R1, R2, R4 and R5 are methyl groups, R3 and R6 are hydrogen, and X is bromine;

[0164]

[0165] A mixture of α-diimine ligand L1-3 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25 ° C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni6. (0.24 g, 90% yield)

[0166] Embodiment 15

[0167] This embodiment provides an α-diimine nickel complex Ni7, wherein R1, R2, R4 and R5 are methyl groups, R3 and R6 are hydrogen, and X is bromine;

[0168]

[0169] A mixture of catalyst Ni6 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni7. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 9.

[0170] Example 16

[0171] This embodiment provides an α-diimine palladium complex Pd6, R1, R2, R4 and R5 are methyl groups, and R3 and R6 are hydroxyl groups;

[0172]

[0173] A mixture of α-diimine ligand L1-3 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd6 (0.24 g, 90% yield).

[0174] Embodiment 17

[0175] This embodiment provides an α-diimine palladium complex Pd7, R1, R2, R4 and R5 are methyl groups, and R3 and R6 are hydroxyl groups;

[0176]

[0177] A mixture of catalyst Pd6 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd7. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 28.

[0178] Embodiment 18

[0179] This embodiment provides an α-diimine ligand L1-4, wherein R1, R2, R4 and R5 are phenyl groups, and R3 and R6 are hydrogen;

[0180]

[0181] Norbornene-4,5-dione (0.2853 g, 2.336 mmol) and 2,6-diphenylaniline (1.1462 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.9300 g, 65% yield).

[0182] Embodiment 19

[0183] This embodiment provides an α-diimine nickel complex Ni8, wherein R1, R2, R4 and R5 are phenyl groups, R3 and R6 are hydrogen, and X is bromine;

[0184]

[0185] A mixture of α-diimine ligand L1-4 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni8 (0.24 g, 90% yield).

[0186] Embodiment 20

[0187] This embodiment provides an α-diimine nickel complex Ni9, wherein R1, R2, R4 and R5 are phenyl groups, R3 and R6 are hydrogen, and X is bromine;

[0188]

[0189] A mixture of catalyst Ni8 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni9. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 9.

[0190] Embodiment 21

[0191] This embodiment provides an α-diimine palladium complex Pd8, R1, R2, R4 and R5 are phenyl, R3 and R6 are hydrogen;

[0192]

[0193] A mixture of α-diimine ligand L1-4 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd8 (0.24 g, 90% yield).

[0194] Embodiment 22

[0195] This embodiment provides an α-diimine palladium complex Pd9, R1, R2, R4 and R5 are phenyl, R3 and R6 are hydrogen;

[0196]

[0197] A mixture of catalyst Pd8 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd9. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 39.

[0198] Embodiment 23

[0199] This embodiment provides an α-diimine ligand L1-5, wherein R1, R2, R4 and R5 are diphenylmethyl groups, and R3 and R6 are methyl groups;

[0200]

[0201] Norbornene-4,5-dione (0.2853 g, 2.336 mmol) and 4-methyl-2,6-diphenylmethylaniline (0.8283 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. The volatiles were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.1164 g, yield 11%).

[0202] Embodiment 24

[0203] This embodiment provides an α-diimine nickel complex Ni10, wherein R1, R2, R4 and R5 are diphenylmethyl, R3 and R6 are methyl; X is bromine;

[0204]

[0205] A mixture of α-diimine ligand L1-5 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni10 (0.24 g, 90% yield).

[0206] Embodiment 25

[0207] This embodiment provides an α-diimine nickel complex Ni11, wherein R1, R2, R4 and R5 are diphenylmethyl, R3 and R6 are methyl; X is bromine;

[0208]

[0209] A mixture of catalyst Ni10 (0.2 g, 0.30 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 5 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 20 mL of hexane, filtered and dried to obtain a brick red solid, namely Ni11. (196 mg, 98% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 5.

[0210] Embodiment 26

[0211] This embodiment provides an α-diimine palladium complex Pd10, R1, R2, R4 and R5 are diphenylmethyl, and R3 and R6 are methyl;

[0212]

[0213] A mixture of α-diimine ligand L1-5 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd10 (0.24 g, 90% yield).

[0214] Embodiment 27

[0215] This embodiment provides an α-diimine palladium complex Pd11, R1, R2, R4 and R5 are diphenylmethyl, and R3 and R6 are methyl;

[0216]

[0217] A mixture of catalyst Pd10 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd11. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 39.

[0218] Embodiment 28

[0219] This embodiment provides an α-diimine ligand L1-6, wherein R1, R2, R3, R4, R5 and R6 are methyl groups;

[0220]

[0221] Norbornene-4,5-dione (0.2853 g, 2.336 mmol) and 2,4,6-trimethylaniline (1.1462 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. The volatiles were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.9300 g, 65% yield).

[0222] Embodiment 29

[0223] This embodiment provides an α-diimine nickel complex Ni12, wherein R1, R2, R3, R4, R5 and R6 are methyl groups; X is bromine;

[0224]

[0225] A mixture of α-diimine ligand L1-6 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni23. (0.24 g, 90% yield).

[0226] Embodiment 30

[0227] This embodiment provides an α-diimine nickel complex Ni13, wherein R1, R2, R3, R4, R5 and R6 are methyl groups; X is bromine;

[0228]

[0229] A mixture of catalyst Ni12 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni13. (190 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 12.

[0230] Embodiment 31

[0231] This embodiment provides an α-diimine palladium complex Pd12, R1, R2, R3, R4, R5 and R6 are methyl groups;

[0232]

[0233] A mixture of α-diimine ligand L1-6 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25 ° C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd12. (0.24 g, 90% yield).

[0234] Embodiment 32

[0235] This embodiment provides an α-diimine palladium complex Pd13, R1, R2, R3, R4, R5 and R6 are methyl groups;

[0236]

[0237] A mixture of catalyst Pd12 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd13. (190 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 32.

[0238] Embodiment 33

[0239] This embodiment provides an α-diimine ligand L1-7, R1 and R4 are hydrogen, R3, R4, R5 and R6 are fluorine;

[0240]

[0241] Norbornene-4,5-dione (0.2853 g, 2.336 mmol) and 2,4-difluoroaniline (0.5662 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. The volatiles were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.5100 g, 60% yield).

[0242] Embodiment 34

[0243] This embodiment provides an α-diimine nickel complex Ni14, R1 and R4 are hydrogen, R3, R4, R5 and R6 are fluorine; X is bromine;

[0244]

[0245] A mixture of α-diimine ligand L1-7 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25 ° C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni14. (0.24 g, 90% yield)

[0246] Embodiment 35

[0247] This embodiment provides an α-diimine nickel complex Ni15, R1 and R4 are hydrogen, R3, R4, R5 and R6 are fluorine; X is bromine;

[0248]

[0249] A mixture of catalyst Ni14 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni15. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 9.

[0250] Embodiment 36

[0251] This embodiment provides an α-diimine palladium complex Pd14, R1 and R4 are hydrogen, and R3, R4, R5 and R6 are fluorine;

[0252]

[0253] A mixture of α-diimine ligand L1-7 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd14. (0.24 g, 90% yield).

[0254] Embodiment 37

[0255] This embodiment provides an α-diimine palladium complex Pd15, R1 and R4 are hydrogen, and R3, R4, R5 and R6 are fluorine;

[0256]

[0257] A mixture of catalyst Pd19 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd15. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 39.

[0258] Embodiment 38

[0259] This embodiment provides an α-diimine ligand L1-8, wherein R1, R2, R4 and R5 are methyl groups, and R3 and R6 are methoxy groups;

[0260]

[0261] Norbornene-4,5-dione (0.2853 g, 2.336 mmol) and 2,6-dimethyl-4-methoxyaniline (0.6317 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.5227 g, 57% yield).

[0262] Embodiment 39

[0263] This embodiment provides an α-diimine nickel complex Ni16, wherein R1, R2, R4 and R5 are methyl groups, R3 and R6 are methoxy groups; X is bromine;

[0264]

[0265] A mixture of α-diimine ligand L1-8 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, the mixture was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid (0.24 g, 90% yield).

[0266] Embodiment 40

[0267] This embodiment provides an α-diimine nickel complex Ni17, R1, R2, R4 and R5 are methyl groups, R3 and R6 are methoxy groups; X is bromine;

[0268]

[0269] A mixture of catalyst Ni17 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni17. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 8.

[0270] Embodiment 41

[0271] This embodiment provides an α-diimine palladium complex Pd16, R1, R2, R4 and R5 are methyl groups, and R3 and R6 are methoxy groups;

[0272]

[0273] A mixture of α-diimine ligand L1-8 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd16 (0.24 g, 90% yield).

[0274] Embodiment 42

[0275] This embodiment provides an α-diimine palladium complex Pd17, R1, R2, R4 and R5 are methyl groups, and R3 and R6 are methoxy groups;

[0276]

[0277] A mixture of catalyst Pd16 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd17. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 28.

[0278] Embodiment 43

[0279] This embodiment provides an α-diimine ligand L1-9, R1 and R4 are hydrogen, R3, R4, R5 and R6 are chlorine;

[0280]

[0281] Norbornene-4,5-dione (0.2853 g, 2.336 mmol) and 2,4-dichloroaniline (0.5662 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. The volatiles were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.5100 g, 60% yield).

[0282] Embodiment 44

[0283] This embodiment provides an α-diimine nickel complex Ni18, R1 and R4 are hydrogen, R3, R4, R5 and R6 are chlorine; X is bromine;

[0284]

[0285] A mixture of α-diimine ligand L1-9 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25 ° C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni18. (0.24 g, 90% yield)

[0286] Embodiment 45

[0287] This embodiment provides an α-diimine nickel complex Ni19, R1 and R4 are hydrogen, R3, R4, R5 and R6 are chlorine; X is bromine;

[0288]

[0289] A mixture of catalyst Ni18 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni19. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 9.

[0290] Embodiment 46

[0291] This embodiment provides an α-diimine palladium complex Pd18, R1 and R4 are hydrogen, and R3, R4, R5 and R6 are chlorine;

[0292]

[0293] A mixture of α-diimine ligand L1-9 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd18 (0.24 g, 90% yield).

[0294] Embodiment 47

[0295] This embodiment provides an α-diimine palladium complex Pd19, R1 and R4 are hydrogen, R3, R4, R5 and R6 are chlorine;

[0296]

[0297] A mixture of catalyst Pd18 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd19. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 39.

[0298] Embodiment 48

[0299] This embodiment provides an α-diimine ligand L1-10, wherein R1, R2, R4 and R5 are hydrogen, and R3 and R6 are methoxy;

[0300]

[0301] Norbornene-4,5-dione (0.2853 g, 2.336 mmol) and 4-methoxyaniline (0.6317 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. The volatiles were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.5227 g, 57% yield).

[0302] Embodiment 49

[0303] This embodiment provides an α-diimine nickel complex Ni20, wherein R1, R2, R4 and R5 are hydrogen, R3 and R6 are methoxy groups; X is bromine;

[0304]

[0305] A mixture of α-diimine ligand L1-10 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, the mixture was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid (0.24 g, 90% yield).

[0306] Embodiment 50

[0307] This embodiment provides an α-diimine nickel complex Ni21, wherein R1, R2, R4 and R5 are hydrogen, R3 and R6 are methoxy groups; X is bromine;

[0308]

[0309] A mixture of catalyst Ni20 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni21. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 8.

[0310] Embodiment 51

[0311] This embodiment provides an α-diimine palladium complex Pd20, R1, R2, R4 and R5 are hydrogen, R3 and R6 are methoxy;

[0312]

[0313] A mixture of α-diimine ligand L1-10 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd20 (0.24 g, 90% yield).

[0314] Embodiment 52

[0315] This embodiment provides an α-diimine palladium complex Pd21, R1, R2, R4 and R5 are hydrogen, R3 and R6 are methoxy;

[0316]

[0317] A mixture of catalyst Pd20 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd21. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 28.

[0318] Embodiment 53

[0319] This embodiment provides an α-diimine ligand L2-1, wherein R1, R2, R4 and R5 are methyl groups, and R3 and R6 are hydrogen;

[0320]

[0321] Cyclooctene-5,6-dione (0.3228 g, 2.336 mmol) and 2,6-dimethylaniline (0.5662 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.5152 g, 58% yield).

[0322] Embodiment 54

[0323] This embodiment provides an α-diimine nickel complex Ni22, wherein R1, R2, R4 and R5 are methyl groups, R3 and R6 are hydrogen, and X is bromine;

[0324]

[0325] A mixture of α-diimine ligand L2-1 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni22. (0.24 g, 90% yield).

[0326] Embodiment 55

[0327] This embodiment provides an α-diimine nickel complex Ni23, R1, R2, R4 and R5 are methyl, R3 and R6 are hydrogen; X is bromine;

[0328]

[0329] A mixture of catalyst Ni22 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni23. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 13.

[0330] Embodiment 56

[0331] This embodiment provides an α-diimine palladium complex Pd22, R1, R2, R4 and R5 are methyl, R3 and R6 are hydrogen;

[0332]

[0333] A mixture of α-diimine ligand L2-1 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd22 (0.24 g, 90% yield).

[0334] Embodiment 57

[0335] This embodiment provides an α-diimine palladium complex Pd23, R1, R2, R4 and R5 are methyl, R3 and R6 are hydrogen;

[0336]

[0337] A mixture of catalyst Pd22 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd23. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 28.

[0338] Embodiment 58

[0339] This embodiment provides an α-diimine ligand L2-2, wherein R1, R2, R4 and R5 are isopropyl, and R3 and R6 are hydrogen;

[0340]

[0341] Cyclooctene-5,6-dione (0.3228 g, 2.336 mmol) and 2,6-diisopropylaniline (0.8283 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.7252 g, 63% yield).

[0342] Embodiment 59

[0343] This embodiment provides an α-diimine nickel complex Ni24, R1, R2, R4 and R5 are isopropyl, R3 and R6 are hydrogen; X is bromine;

[0344]

[0345] A mixture of α-diimine ligand L2-2 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni24. (0.24 g, 90% yield).

[0346] Embodiment 60

[0347] This embodiment provides an α-diimine nickel complex Ni25, R1, R2, R4 and R5 are isopropyl, R3 and R6 are hydrogen; X is bromine;

[0348]

[0349] A mixture of catalyst Ni24 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni25. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 13.

[0350] Embodiment 61

[0351] This embodiment provides an α-diimine palladium complex Pd24, R1, R2, R4 and R5 are isopropyl, R3 and R6 are hydrogen;

[0352]

[0353] A mixture of α-diimine ligand L2-2 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd24. (0.24 g, 90% yield).

[0354] Embodiment 62

[0355] This embodiment provides an α-diimine palladium complex Pd25, R1, R2, R4 and R5 are isopropyl, R3 and R6 are hydrogen;

[0356]

[0357] A mixture of catalyst Pd24 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd25. (190 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 32.

[0358] Embodiment 63

[0359] This embodiment provides an α-diimine ligand L2-3, wherein R1, R2, R4 and R5 are methyl groups, and R3 and R6 are hydroxy groups;

[0360]

[0361] Cyclooctene-5,6-dione (0.3228 g, 2.336 mmol) and 2,6-dimethyl-4-hydroxy-aniline (0.6317 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.3912 g, yield was 41%).

[0362] Embodiment 64

[0363] This embodiment provides an α-diimine nickel complex Ni26, wherein R1, R2, R4 and R5 are methyl groups, R3 and R6 are hydroxy groups; X is bromine;

[0364]

[0365] A mixture of α-diimine ligand L2-3 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni26. (0.24 g, 90% yield).

[0366] Embodiment 65

[0367] This embodiment provides an α-diimine nickel complex Ni27, wherein R1, R2, R4 and R5 are methyl groups, R3 and R6 are hydroxy groups; X is bromine;

[0368]

[0369] A mixture of catalyst Ni26 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni27. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 13.

[0370] Embodiment 66

[0371] This embodiment provides an α-diimine palladium complex Pd26, R1, R2, R4 and R5 are methyl groups, and R3 and R6 are hydroxyl groups;

[0372]

[0373] A mixture of α-diimine ligand L2-3 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd26 (0.24 g, 90% yield).

[0374] Embodiment 67

[0375] This embodiment provides an α-diimine palladium complex Pd27, R1, R2, R4 and R5 are methyl groups, and R3 and R6 are hydroxyl groups;

[0376]

[0377] A mixture of catalyst Pd26 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd27. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 33.

[0378] Embodiment 68

[0379] This embodiment provides an α-diimine ligand L2-4, wherein R1, R2, R4 and R5 are phenyl groups, and R3 and R6 are hydrogen;

[0380]

[0381] Cyclooctene-5,6-dione (0.3228 g, 2.336 mmol) and 2,6-diphenylaniline (1.1462 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (1.014 g, 69% yield).

[0382] Embodiment 69

[0383] This embodiment provides an α-diimine nickel complex Ni28, wherein R1, R2, R4 and R5 are phenyl groups, R3 and R6 are hydrogen, and X is bromine;

[0384]

[0385] A mixture of α-diimine ligand L2-4 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni28 (0.24 g, 90% yield).

[0386] Embodiment 70

[0387] This embodiment provides an α-diimine nickel complex Ni29, wherein R1, R2, R4 and R5 are phenyl groups, R3 and R6 are hydrogen, and X is bromine;

[0388]

[0389] A mixture of catalyst Ni28 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni29. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 9.

[0390] Embodiment 71

[0391] This embodiment provides an α-diimine palladium complex Pd28, R1, R2, R4 and R5 are phenyl, R3 and R6 are hydrogen;

[0392]

[0393] A mixture of α-diimine ligand L2-4 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd28 (0.24 g, 90% yield).

[0394] Embodiment 72

[0395] This embodiment provides an α-diimine palladium complex Pd29, R1, R2, R4 and R5 are phenyl, R3 and R6 are hydrogen;

[0396]

[0397] A mixture of catalyst Pd28 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd29. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 29.

[0398] Embodiment 73

[0399] This embodiment provides an α-diimine ligand L2-5, wherein R1, R2, R4 and R5 are diphenylmethyl groups, and R3 and R6 are methyl groups;

[0400]

[0401] Cyclooctene-5,6-dione (0.3228 g, 2.336 mmol) and 2,6-dibenzhydryl-4-methylaniline (0.5662 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. The volatiles were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.5152 g, 58% yield).

[0402] Embodiment 74

[0403] This embodiment provides an α-diimine nickel complex Ni30, wherein R1, R2, R4 and R5 are diphenylmethyl, R3 and R6 are methyl; X is bromine;

[0404]

[0405] A mixture of α-diimine ligand L2-5 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni30. (0.24 g, 90% yield).

[0406] Embodiment 75

[0407] This embodiment provides an α-diimine nickel complex Ni31, wherein R1, R2, R4 and R5 are diphenylmethyl, R3 and R6 are methyl; X is bromine;

[0408]

[0409] A mixture of catalyst Ni30 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni31. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 13.

[0410] Embodiment 76

[0411] This embodiment provides an α-diimine palladium complex Pd30, R1, R2, R4 and R5 are diphenylmethyl, and R3 and R6 are methyl;

[0412]

[0413] A mixture of α-diimine ligand L2-5 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd30 (0.24 g, 90% yield).

[0414] Embodiment 77

[0415] This embodiment provides an α-diimine palladium complex Pd31, R1, R2, R4 and R5 are diphenylmethyl, and R3 and R6 are methyl;

[0416]

[0417] A mixture of catalyst Pd30 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd31. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 28.

[0418] Embodiment 78

[0419] This embodiment provides an α-diimine ligand L2-6, wherein R1, R2, R4 and R5 are methyl groups, and R3 and R6 are methyl groups;

[0420]

[0421] Cyclooctene-5,6-dione (0.3228 g, 2.336 mmol) and 2,4,6-trimethylaniline (0.5662 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.5152 g, 58% yield).

[0422] Embodiment 79

[0423] This embodiment provides an α-diimine nickel complex Ni32, wherein R1, R2, R4 and R5 are methyl groups, R3 and R6 are methyl groups; X is bromine;

[0424]

[0425] A mixture of α-diimine ligand L2-6 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni32. (0.24 g, 90% yield).

[0426] Embodiment 80

[0427] This embodiment provides an α-diimine nickel complex Ni33, R1, R2, R4 and R5 are methyl groups, R3 and R6 are methyl groups; X is bromine;

[0428]

[0429] A mixture of catalyst Ni32 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni33. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 13.

[0430] Embodiment 81

[0431] This embodiment provides an α-diimine palladium complex Pd32, R1, R2, R4 and R5 are methyl groups, and R3 and R6 are methyl groups;

[0432]

[0433] A mixture of α-diimine ligand L2-6 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25 ° C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd32. (0.24 g, 90% yield).

[0434] Embodiment 82

[0435] This embodiment provides an α-diimine palladium complex Pd33, R1, R2, R4 and R5 are methyl groups, and R3 and R6 are methyl groups;

[0436]

[0437] A mixture of catalyst Pd32 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd33. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 28.

[0438] Embodiment 83

[0439] This embodiment provides an α-diimine ligand L2-7, R1 and R4 are hydrogen, and R3, R4, R5 and R6 are fluorine;

[0440]

[0441] Cyclooctene-5,6-dione (0.3228 g, 2.336 mmol) and 2,4-difluoroaniline (0.5662 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.5152 g, 58% yield).

[0442] Embodiment 84

[0443] This embodiment provides an α-diimine nickel complex Ni34, R1 and R4 are hydrogen, R3, R4, R5 and R6 are fluorine; X is bromine;

[0444]

[0445] A mixture of α-diimine ligand L2-7 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni34. (0.24 g, 90% yield).

[0446] Embodiment 85

[0447] This embodiment provides an α-diimine nickel complex Ni35, R1 and R4 are hydrogen, R3, R4, R5 and R6 are fluorine; X is bromine;

[0448]

[0449] A mixture of catalyst Ni34 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni35. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 13.

[0450] Embodiment 86

[0451] This embodiment provides an α-diimine palladium complex Pd34, R1 and R4 are hydrogen, R3, R4, R5 and R6 are fluorine;

[0452]

[0453] A mixture of α-diimine ligand L2-7 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd34. (0.24 g, 90% yield).

[0454] Embodiment 87

[0455] This embodiment provides an α-diimine palladium complex Pd35, R1 and R4 are hydrogen, R3, R4, R5 and R6 are fluorine;

[0456]

[0457] A mixture of catalyst Pd34 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd35. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 28.

[0458] Embodiment 88

[0459] This embodiment provides an α-diimine ligand L2-8, wherein R1, R2, R4 and R5 are methyl groups, and R3 and R6 are methoxy groups;

[0460]

[0461] Cyclooctene-5,6-dione (0.3228 g, 2.336 mmol) and 4-methoxy-2,6-dimethylaniline (0.8283 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.7252 g, 63% yield).

[0462] Embodiment 89

[0463] This embodiment provides an α-diimine nickel complex Ni36, wherein R1, R2, R4 and R5 are methyl groups, R3 and R6 are methoxy groups; X is bromine;

[0464]

[0465] A mixture of α-diimine ligand L2-8 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni36. (0.24 g, 90% yield).

[0466] Embodiment 90

[0467] This embodiment provides an α-diimine nickel complex Ni37, R1, R2, R4 and R5 are methyl groups, R3 and R6 are methyl groups; X is bromine;

[0468]

[0469] A mixture of catalyst Ni36 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni37. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 13.

[0470] Embodiment 91

[0471] This embodiment provides an α-diimine palladium complex Pd36, R1, R2, R4 and R5 are methyl groups, and R3 and R6 are methoxy groups;

[0472]

[0473] A mixture of α-diimine ligand L2-8 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd36 (0.24 g, 90% yield).

[0474] Embodiment 92

[0475] This embodiment provides an α-diimine palladium complex Pd37, R1, R2, R4 and R5 are methyl groups, and R3 and R6 are methoxy groups;

[0476]

[0477] A mixture of catalyst Pd36 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd37. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 28.

[0478] Embodiment 93

[0479] This embodiment provides an α-diimine ligand L2-9, wherein R1 and R4 are hydrogen, and R3, R4, R5 and R6 are chlorine;

[0480]

[0481] Cyclooctene-5,6-dione (0.3228 g, 2.336 mmol) and 2,4-dichloroaniline (0.5662 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.5152 g, 58% yield).

[0482] Embodiment 94

[0483] This embodiment provides an α-diimine nickel complex Ni38, R1 and R4 are hydrogen, R3, R4, R5 and R6 are chlorine; X is bromine;

[0484]

[0485] A mixture of α-diimine ligand L2-9 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni38. (0.24 g, 90% yield).

[0486] Embodiment 95

[0487] This embodiment provides an α-diimine nickel complex Ni39, R1 and R4 are hydrogen, R3, R4, R5 and R6 are chlorine; X is bromine;

[0488]

[0489] A mixture of catalyst Ni38 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni39. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 13.

[0490] Embodiment 96

[0491] This embodiment provides an α-diimine palladium complex Pd38, R1 and R4 are hydrogen, R3, R4, R5 and R6 are chlorine;

[0492]

[0493] A mixture of α-diimine ligand L2-9 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd38 (0.24 g, 90% yield).

[0494] Embodiment 97

[0495] This embodiment provides an α-diimine palladium complex Pd39, R1 and R4 are hydrogen, R3, R4, R5 and R6 are chlorine;

[0496]

[0497] A mixture of catalyst Pd38 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd39. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 28.

[0498] Embodiment 98

[0499] This embodiment provides an α-diimine ligand L2-10, wherein R1, R2, R4 and R5 are hydrogen, and R3 and R6 are methoxy;

[0500]

[0501] Cyclooctene-5,6-dione (0.3228 g, 2.336 mmol) and 4-methoxy-2,6-dimethylaniline (0.8283 g, 4.672 mmol) were dissolved in a mixture of methanol (2.5 mL) and formic acid (0.25 mL). The mixture was stirred at room temperature for 24 h. Volatile substances were removed, methanol (1.0 mL) was added, and the mixture was cooled to -78 ° C. The solid formed was filtered and dried (0.7252 g, 63% yield).

[0502] Embodiment 99

[0503] This embodiment provides an α-diimine nickel complex Ni40, wherein R1, R2, R4 and R5 are hydrogen, R3 and R6 are methoxy groups; X is bromine;

[0504]

[0505] A mixture of α-diimine ligand L2-10 (0.17 g, 0.41 mmol) and (DME)NiBr2 (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25°C for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Ni40. (0.24 g, 90% yield).

[0506] Embodiment 100

[0507] This embodiment provides an α-diimine nickel complex Ni41, wherein R1, R2, R4 and R5 are hydrogen, R3 and R6 are methoxy groups; X is bromine;

[0508]

[0509] A mixture of catalyst Ni40 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Ni41. (188 mg, 94% yield). The catalyst is a macromolecular nickel catalyst with a polymerization degree n of 13.

[0510] Embodiment 101

[0511] This embodiment provides an α-diimine palladium complex Pd40, R1, R2, R4 and R5 are hydrogen, R3 and R6 are methoxy;

[0512]

[0513] A mixture of α-diimine ligand L2-10 (0.17 g, 0.41 mmol) and (COD)PdMeCl (130 mg, 0.42 mmol) was stirred in 20 mL of dichloromethane at 25° C. for 72 hours. After the reaction was completed, it was filtered and the solvent was evaporated under reduced pressure to obtain a yellow-green solid, namely Pd25. (0.24 g, 90% yield).

[0514] Embodiment 102

[0515] This embodiment provides an α-diimine palladium complex Pd41, R1, R2, R4 and R5 are hydrogen, R3 and R6 are methoxy;

[0516]

[0517] A mixture of catalyst Pd40 (0.5 g, 0.76 mmol) and Grubbs II catalyst (6.4 mg, 7.5 μmol) was stirred in 10 mL of dichloromethane at room temperature for 12 hours. After the reaction was completed, the solution was poured into 40 mL of hexane, filtered and dried to obtain a reddish brown solid, namely Pd41. (188 mg, 94% yield). The catalyst is a macromolecular palladium catalyst with a polymerization degree n of 28.

[0518] Application Example 1-Ethylene Homopolymerization Catalyzed by Nickel Catalyst

[0519] First, a 350 mL glass pressure reactor connected to a high-pressure gas pipeline was vacuum dried at 90°C for at least 1 hour. Then the reactor was adjusted to 30°C, 50°C, 70°C and 90°C, 98 mL of toluene and 500 equivalents of a co-catalyst (MAO) were added to the reactor under an inert atmosphere, and then a nickel catalyst (1 μmol) was dissolved in 2 mL of dichloromethane or chloroform and injected into the polymerization system through a syringe. Under rapid stirring (450 rpm or more), ethylene was introduced and maintained at 8 atmospheres. After 30 minutes, the pressure reactor was emptied, a large amount of acidic methanol (or ethanol) (5% or more hydrochloric acid alcohol solution) solution was added to quench the polymerization reaction, the polymer was filtered, and dried in a vacuum oven to constant weight.

[0520] The data on the effect of different temperatures during MAO activation and the degree of polymerization of the macromolecular nickel catalyst I on ethylene polymerization are shown in Table 1 below (all data are based on at least two parallel tests (unless otherwise stated). Activity: 10 6 gmol -1 h -1 The unit is M n is the number average molecular weight, polymer molecular weight and molecular weight distribution determined by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Degree of branching = number of branches per 1000 carbons, determined by H NMR spectroscopy).

[0521] Table 1

[0522]

[0523]

[0524] From the data in Table 1, it can be seen that under the same conditions, as the degree of polymerization of Ni3~Ni5 catalysts increases, the activity of catalyzing ethylene homopolymerization increases significantly, and the molecular weight increases significantly; and the polymerization reaction of the same catalyst decreases with increasing temperature, the activity decreases, the molecular weight decreases, and the degree of branching increases. The single molecule catalyst Ni3 loses its activity at 90℃, but the macromolecular nickel catalysts Ni4 and Ni5 still have high activity at 90℃.

[0525] The data of the effects of different temperatures during MAO activation and the axial steric hindrance of the macromolecular nickel catalyst I on ethylene polymerization are shown in Table 2 below (all data are based on at least two parallel tests (unless otherwise stated). Activity: 10 6 gmol -1 h -1 The unit is M nis the number average molecular weight, polymer molecular weight and molecular weight distribution determined by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Degree of branching = number of branches per 1000 carbons, determined by H NMR spectroscopy).

[0526] Table 2

[0527]

[0528] From the data in Table 2, it can be seen that under the same conditions, as the axial steric hindrance of Ni2, Ni9, and Ni5 catalysts increases, the activity of catalyzing ethylene homopolymerization increases significantly, and the molecular weight increases significantly; and for the polymerization reaction of the same catalyst, as the temperature increases, the activity decreases, the molecular weight decreases, and the degree of branching increases. Application Example 2 - Nickel Catalyzed Ethylene Homopolymerization

[0529] First, a 350 mL glass pressure reactor connected to a high-pressure gas pipeline was vacuum dried at 90°C for at least 1 hour. The reactor was then adjusted to 30°C, 50°C, 70°C and 90°C, 98 mL of toluene and 500 equivalents of a cocatalyst (Et2AlCl) were added to the reactor under an inert atmosphere, and then a nickel catalyst (1 μmol) was dissolved in 2 mL of dichloromethane or chloroform and injected into the polymerization system through a syringe. Under rapid stirring (450 rpm or more), ethylene was introduced and maintained at 8 atmospheres. After 30 minutes, the pressure reactor was emptied, a large amount of acidic methanol (or ethanol) (5% or more of hydrochloric acid alcohol solution) solution was added to quench the polymerization reaction, the polymer was filtered, and dried in a vacuum oven to constant weight.

[0530] The data on the effect of different temperatures and the degree of polymerization of the macromolecular nickel catalyst I on ethylene polymerization during Et2AlCl activation are shown in Table 3 below (all data are based on at least two parallel tests (unless otherwise stated). Activity: 10 6 g mol -1 h -1 The unit is M n is the number average molecular weight, polymer molecular weight and molecular weight distribution determined by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Degree of branching = number of branches per 1000 carbons, determined by H NMR spectroscopy).

[0531] Table 3

[0532]

[0533] From the data in Table 3, it can be seen that under the same conditions, as the degree of polymerization of Ni3 to Ni5 catalysts increases, the activity of catalyzing ethylene homopolymerization increases significantly, and the molecular weight increases significantly; and the polymerization reaction of the same catalyst decreases with increasing temperature, the activity decreases, the molecular weight decreases, and the degree of branching increases. The single molecule catalyst Ni3 loses its activity at 90°C, but the macromolecular nickel catalysts Ni4 and Ni5 still have high activity at 90°C.

[0534] The hydrogen spectrum of the polymer prepared corresponding to No. 11 in Table 3 is as follows Figure 2 As shown, it can be seen that the obtained polymer has a lot of branching and may be an elastomer with good performance.

[0535] The stress-strain test was performed on the polymers prepared corresponding to No. 5, 9, and 10 in Table 3, and the test method was as follows:

[0536] Polymer strips with a length of 15 mm, a width of 2 mm, and a thickness of 1 mm were prepared and cut out, and the GB-T1040.3 2006 tensile test of 100 N was carried out.

[0537] Test results such as Figure 3 As shown, it can be seen that Ni5 can prepare polyethylene elastomers with higher elongation at break than Ni4, and the branching degree of the elastomer can be adjusted by temperature. The higher the temperature, the higher the branching degree.

[0538] The elastic recovery test was performed on the polymer prepared corresponding to No. 5 in Table 3, and the test method was as follows:

[0539] Prepare and cut polymer strips with a length of 15 mm, a width of 2 mm, and a thickness of 1 mm, and perform a fixed cycle of 100 N according to GB-T1040.3 2006.

[0540] Test results such as Figure 4 As shown, it can be seen that sample No. 5 in Table 3 has good elastic recovery performance, and the elastic recovery rate reaches 63%.

[0541] The data of the effect of different temperatures and axial steric hindrance of macromolecular nickel catalyst I on ethylene polymerization during Et2AlCl activation are shown in Table 4 below (all data are based on at least two parallel tests (unless otherwise stated). 6 g mol -1 h -1 The unit is M n is the number average molecular weight, polymer molecular weight and molecular weight distribution determined by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Degree of branching = number of branches per 1000 carbons, determined by H NMR spectroscopy).

[0542] Table 4

[0543]

[0544] It can be seen from the data in Table 4 that, under the same conditions, as the axial steric hindrance of Ni2, Ni9, and Ni5 catalysts increases, the activity of catalyzing ethylene homopolymerization increases significantly, and the molecular weight increases significantly; and for the polymerization reaction of the same catalyst, as the temperature increases, the activity decreases, the molecular weight decreases, and the degree of branching increases.

[0545] Application Example 3- Ethylene Homopolymerization Catalyzed by Palladium Catalyst

[0546] First, a 350 mL glass pressure reactor connected to a high pressure gas line was vacuum dried at 90°C for at least 1 hour. The reactor was then adjusted to 30°C, 50°C, 70°C and 90°C, 98 mL of toluene and 1.2 μmol of NaBArF were added to the reactor under an inert atmosphere, and then a palladium catalyst (1 μmol) was dissolved in 2 mL of dichloromethane or chloroform and injected into the polymerization system through a syringe. Under rapid stirring (750 rpm or more), ethylene was introduced and maintained at 8 atmospheres. After 30 minutes, the pressure reactor was emptied, a large amount of acidic methanol (or ethanol) (5% or more of hydrochloric acid alcohol solution) solution was added to quench the polymerization reaction, the polymer was filtered, and dried in a vacuum oven to constant weight.

[0547] The data on the effect of temperature on the macromolecular α-diimine palladium catalyst of the structure shown in Formula Ⅱ on ethylene polymerization are shown in Table 5 below (all data are based on at least two parallel tests (unless otherwise stated). Activity: 10 6 gmol -1 h -1 The unit is M n is the number average molecular weight, polymer molecular weight and molecular weight distribution determined by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Degree of branching = number of branches per 1000 carbons, determined by H NMR spectroscopy).

[0548] Table 5

[0549]

[0550] It can be seen from the data in Table 5 that under the same conditions, the polymerization activity of the macromolecular palladium catalyst is higher than that of the monomeric palladium catalyst, and the prepared polymer has a higher molecular weight, a lower degree of branching, and a narrower molecular weight distribution.

[0551] Application Example 4 - Scale-up experiment of ethylene polymerization catalyzed by the macromolecular nickel catalyst of formula I activated by methylaluminoxane (MAO)

[0552] First, a 20L industrial polymerization kettle connected to a high-pressure gas pipeline was vacuum dried at 90°C for at least 1 hour. Then the temperature of the polymerization kettle was adjusted to 65°C, 13L of n-hexane and 500eq MAO were added to the reactor under an inert atmosphere, and then a specified amount of nickel catalyst was dissolved in a specific equivalent of dichloromethane (1mL of dichloromethane was used to dissolve each 1mol of catalyst) and injected into the polymerization system through a syringe. Under rapid stirring, ethylene was introduced to quickly raise the pressure to 20 bar. After 1 hour, the pressure in the kettle was vented, and after the reaction solution was placed in a stainless steel barrel, 13L of acidic ethanol (ethanol solution containing 5% hydrochloric acid by mass) was added to quench the polymerization reaction, the polymer was separated, and dried in a vacuum oven to constant weight. The test results are shown in Table 6 below (all data are based on at least two parallel tests (unless otherwise stated). Activity: 10 6 g mol -1 h -1 The unit is M n is the number average molecular weight, polymer molecular weight and molecular weight distribution determined by GPC in 1,2,4-trichlorobenzene at 150°C, relative to polystyrene standards. Degree of branching = number of branches per 1000 carbons, determined by H NMR spectroscopy).

[0553] Table 6

[0554]

[0555] From the data in Table 6, it can be seen that under the conditions of scale-up, the macromolecular Ni5 catalyst can prepare highly branched polyethylene elastomers with high activity, and the highest activity is up to 12×10 6 g mol -1 h -1 , i.e. 18kg PE / g Cat In contrast, the single-molecule catalyst Ni3 has lower activity and molecular weight.

[0556] It should be noted that the above-mentioned acidic ethanol can also be replaced by acidic methanol (methanol solution containing 5% hydrochloric acid by mass).

[0557] In summary, the present invention has the following advantages:

[0558] (1) Innovation in catalyst structure: A class of α-diimine ligands and nickel and palladium catalysts were synthesized, which have double bonds in the skeleton and a special structure;

[0559] (2) Innovative synthesis route: The intracyclic double bonds on the ligand skeleton of the macromolecular catalyst can be formed into macromolecular ligands or catalysts through ring-opening metathesis polymerization, which is highly innovative;

[0560] (3) Excellent catalyst performance: A class of macromolecular α-diimine nickel and palladium catalysts were synthesized through ring-opening metathesis polymerization, which significantly improved the polymerization activity and polymer molecular weight. The activity was increased by up to 7.5 times (No. 9 vs. No. 1 in Table 4), and the molecular weight was increased by 85 times (No. 9 vs. No. 1 in Table 3);

[0561] (4) The prepared polymer has excellent performance: the preparation of high molecular weight polyethylene elastomer (380,000) with a certain degree of branching (48-111 / 1000C) has been achieved. This type of elastomer is low-cost to prepare with ethylene as the only raw material, and has excellent tensile and recovery properties, and has great application prospects.

[0562] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A macromolecular α-diimine nickel and palladium catalyst, characterized in that: Having the structure shown in formula Ⅰ or Ⅱ: Among them, R 1 , R 2 , R 4 and R 5 Each is independently selected from substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C6-C30 aryl; R 3 and R 6 Each is independently selected from hydrogen, hydroxy, halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C1-C6 alkoxy; M is nickel or palladium; X is halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C6-C30 aryl; The value of n is 2 to 1000.

2. The macromolecular α-diimine nickel and palladium catalyst according to claim 1, characterized in that: The R 1 , R 2 , R 4 and R 5 Each is independently selected from substituted or unsubstituted C1-C4 alkyl, substituted or unsubstituted C6-C20 aryl; R 3 and R 6 Each is independently selected from hydrogen, hydroxy, halogen, substituted or unsubstituted C1-C4 alkyl, substituted or unsubstituted C1-C4 alkoxy; X is halogen, substituted or unsubstituted C1-C4 alkyl, or substituted or unsubstituted C6-C20 aryl.

3. The macromolecular α-diimine nickel and palladium catalyst according to claim 1 or 2, characterized in that: The R 1 , R 2 , R 4 and R 5 Each is independently selected from methyl, phenyl, isopropyl or diphenylmethyl; R 3 and R 6 are each independently selected from hydrogen, methyl, hydroxy, halogen or methoxy; X is halogen, substituted or unsubstituted C1-C3 alkyl, or substituted or unsubstituted C6-C18 aryl.

4. The macromolecular α-diimine nickel and palladium catalyst according to claim 1, characterized in that: The macromolecular α-diimine nickel and palladium catalyst is selected from any one of formulas Ⅰ-1 to Ⅰ-10 or formulas Ⅱ-1 to Ⅱ-10:

5. A method for preparing a macromolecular α-diimine nickel and palladium catalyst as claimed in any one of claims 1 to 4, characterized in that: The preparation method of the macromolecular α-diimine nickel and palladium catalyst having the structure shown in formula I or formula II comprises: S1-1: mixing norbornene dione or cyclooctenedione with a substituted aromatic amine represented by formula A and reacting them to obtain a compound represented by formula L1 or formula L2; S2-1: mixing and reacting the compound represented by formula L1 or formula L2 with a nickel source or a palladium source to obtain a compound represented by formula C1 or formula C2; S3-1: polymerizing the compound represented by formula C1 or formula C2 in the presence of a catalyst to obtain a macromolecular α-diimine nickel or palladium catalyst represented by formula I or formula Ⅰ; or S1-2: According to the method of S1-1, a compound represented by formula L1 or formula L2 is obtained; S2-2: polymerizing the compound represented by formula L1 or formula L2 in the presence of a catalyst to obtain a compound represented by formula L1-P or L2-P; S3-2: mixing and reacting the compound represented by formula L1-P or L2-P with a nickel source or a palladium source to obtain a macromolecular α-diimine nickel and palladium catalyst represented by formula I or formula Ⅰ; 6. The preparation method according to claim 5, characterized in that: The molar ratio of the norbornene dione or cyclooctenedione to the substituted aromatic amine represented by formula A is 1:1 to 1:20; The molar ratio of the compound represented by Formula L1 or Formula L2 to the nickel source or palladium source is 1:1 to 1:10; The molar ratio of the compound represented by formula C1 or formula C2 to the catalyst is 10:1 to 1000:1; The molar ratio of the compound represented by formula L1 or formula L2 to the catalyst is 10:1 to 1000:1; The molar ratio of the compound represented by formula L1-P or formula L2-P to the nickel source or palladium source is 1:n.

7. The preparation method according to claim 5 or 6, characterized in that: The reaction temperature in step S1-1 is 20 to 80° C., and the reaction time is 2 to 10 hours; The reaction temperature in step S2-1 or step S3-2 is independently 15 to 30° C., and the reaction time is independently 40 to 90 h. The polymerization temperature in step S2-2 or step S3-1 is independently 15 to 30° C., and the polymerization time is independently 5 to 20 hours.

8. The preparation method according to any one of claims 5 to 7, characterized in that The nickel source is selected from ethylene glycol dimethyl ether nickel bromide and / or ethylene glycol dimethyl ether nickel chloride; The palladium source is selected from chloro(1,5-cyclooctadiene)methylpalladium(II); The catalyst is selected from any one or more of a Grubbs I catalyst, a Grubbs II catalyst, a Grubbs III catalyst, a Hoveyda-Grubbs I catalyst or a Hoveyda-Grubbs II catalyst.

9. Use of the macromolecular α-diimine nickel or palladium catalyst according to any one of claims 1 to 4 or the macromolecular α-diimine nickel or palladium catalyst prepared by the preparation method according to any one of claims 5 to 8 in ethylene polymerization.

10. The use according to claim 9, characterized in that: The application temperature of the macromolecular α-diimine nickel and palladium catalyst is ≥ 0°C.

Citation Information

Patent Citations

  • Novel catalyst systems and their use for metathesis reactions

    CN101024200A

  • Large steric hindrance diimine nickel catalyst and ligand thereof, and preparation method and application thereof

    CN109608507A

  • Fluorine-containing alpha-diimine nickel coordination compounds for preparing polyolefin elastomer, intermediate, preparation method and application thereof

    CN111303215A

  • Macromolecular diimine nickel-palladium catalyst and application thereof

    CN115141116A

  • Novel catalyst systems and a process for reacting chemical compounds in the presence of said catalyst systems