Vinyl silicone oil as well as preparation method and application thereof
By preparing vinyl silicone oil under vacuum dehydration, using a combination reaction of alkaline catalyst and silicon hydroxyl control agent, the volatile cyclosiloxane oligomer and silicon hydroxyl component content in vinyl silicone oil in the prior art was solved. The problem is that the oil distillation rate of thermally conductive silicon gels and the environmental protection of the vulcanization process are improved.
Patent Information
- Application Number
- CN202410459528.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-22
AI Technical Summary
There is a problem that the volatile cyclosiloxane oligomer and silicon hydroxyl component content is high in the existing preparation methods of vinyl silicone oil, which affects the oil extraction rate of thermally conductive silicone gels and pollutant emissions during vulcanization.
The alkaline catalyst was prepared under vacuum dehydration conditions, and the dimethylsiloxane ring, vinyl capping agent and silicon hydroxyl control agent were mixed, and then the equilibrium reaction was carried out under dry dehydration gas protection and vacuum conditions. The alkaline catalyst was removed to obtain a vinyl silicone oil with low volatile cyclosiloxane oligomer content and low silicon hydroxyl value.
It effectively reduces the volatile cyclosiloxane oligomer content and silicon hydroxyl value in vinyl silicone oil, improves the oil extraction rate of thermally conductive silicon gel, ensures pollutant control during vulcanization, and ensures safety and environmental protection.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer material synthesis, and specifically relates to vinyl silicone oil and a preparation method and application thereof. Background Art
[0002] Thermally conductive gel is a gel-like thermally conductive material made by stirring, mixing and encapsulating a composite thermally conductive filler made of silicone. This material has some advantages of thermally conductive gaskets and thermally conductive silicone grease, and makes up for the weaknesses of both. Thermally conductive gel inherits the advantages of silicone materials such as good affinity, weather resistance, high and low temperature resistance and good insulation. At the same time, it has strong plasticity and can meet the filling of uneven interfaces and can meet the heat transfer requirements of various applications. This product is widely used in the electronic and electrical industry to make insulation, sealing, heat dissipation materials, etc. Among them, the two-component medium-temperature vulcanized thermally conductive silicone gel has excellent fluidity and easy operation; moderate curing temperature, fast vulcanization speed, good high and low temperature resistance, and excellent electrical insulation performance; after curing, the film is soft, sticky, and has a low oil separation rate; no pollutants are released during the vulcanization process, and it has the advantages of safety and environmental protection.
[0003] Vinyl silicone oil is an important source of base material for thermal conductive gel and the main raw material for addition-type liquid silicone rubber. At present, the preparation process mostly uses dimethylsiloxane cyclopentadiene (DMC) or octamethylcyclotetrasiloxane (D4) as raw materials, vinyl siloxane as end-capping agent, and uses acidic or alkaline catalysts for ring-opening equilibrium reaction. However, the vinyl silicone oil prepared by these methods generally has two problems: (1) It generally contains 1~3% volatile cyclosiloxane oligomers; (2) There is a certain amount of water in the raw materials and reaction system, and the prepared vinyl silicone oil contains a large amount of silanol components. These two major shortcomings will affect the performance of downstream products, making thermal conductive silicone gel prone to silanol condensation cross-linking, unable to achieve a low oil precipitation rate, and unable to achieve the effect of no pollutant release during the vulcanization process. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for preparing vinyl silicone oil, which has the advantages of simple operation and high yield, and can prepare vinyl silicone oil with low volatile cyclosiloxane oligomer content and low silanol value.
[0005] The present invention also provides vinyl silicone oil prepared according to the preparation method.
[0006] The invention also provides a thermally conductive silicone gel.
[0007] According to one aspect of the present invention, a method for preparing vinyl silicone oil is provided, comprising the following steps: S1: Under vacuum dehydration conditions, dimethylsiloxane ring body and alkaline compound are mixed and reacted to prepare an alkaline catalyst; S2: mixing the dimethylsiloxane ring body, the alkaline catalyst and the vinyl end-capping agent, and reacting to obtain a first mixed material; S3: adding a silanol control agent to the first mixed material, and carrying out a balanced reaction for 0.5 to 6 hours to obtain a second mixed material; S4: removing the alkaline catalyst; then degassing under the protection of a dry and dehydrated gas and vacuum conditions, and filtering to obtain the vinyl silicone oil.
[0008] According to a preferred embodiment of the present invention, at least the following beneficial effects are achieved: Raw materials, catalysts and trace amounts of water in the air will lead to a high silanol value in the synthesized vinyl silicone oil, as well as a high content of volatile cyclosiloxane oligomers. The present invention adopts the above-mentioned preparation method to prepare an alkaline catalyst under vacuum dehydration conditions; mix dimethylsiloxane ring body, vinyl end-capping agent and alkaline catalyst, and add a silanol control agent for reaction; and dehydrate under dry dehydration gas protection and vacuum conditions to prepare vinyl silicone oil, which can reduce the silanol value of the finished product and reduce the content of volatile cyclosiloxane oligomers therein.
[0009] The preparation method of the present invention has the advantages of simple operation and high yield, and the vinyl silicone oil prepared by the method has a low content of volatile cyclosiloxane oligomers (≤0.5%) and a low silanol value. The vinyl silicone oil is used for thermally conductive silicone gel, which can effectively improve the oil separation rate of the thermally conductive silicone gel, strictly control the discharge of pollutants in the vulcanization process of the thermally conductive silicone gel, and ensure the safety and environmental protection of the use process.
[0010] In some embodiments of the present invention, the vacuum degree of the vacuum in step S1 is -0.045~-0.095MPa.
[0011] In some embodiments of the present invention, the temperature of the vacuum dehydration in step S1 is ≤90°C.
[0012] In some embodiments of the present invention, the temperature for mixing the dimethylsiloxane ring body and the alkaline compound in step S1 is 60-120° C. and the time is 2-6 hours.
[0013] In some embodiments of the present invention, in step S1, 1 to 10 parts by weight of the dimethylsiloxane ring and 0.1 to 1.0 parts by weight of the basic compound are mixed for reaction.
[0014] In some embodiments of the present invention, the dimethylsiloxane ring body includes at least one of a hexamethyltrisiloxane ring body (D3), an octamethylcyclotetrasiloxane (D4), a decamethylpentasiloxane ring body (D5), a dodecamethylcyclohexasiloxane (D6), and a tetradecamethylcycloheptasiloxane (D7).
[0015] In some embodiments of the present invention, the alkaline compound includes at least one of ethylamine, triethylamine, tetramethylammonium hydroxide, and ethanolamine.
[0016] In some embodiments of the present invention, in step S2, the dimethylsiloxane ring body is first added into a reaction kettle and the temperature is raised to 50-120° C.; then the alkaline catalyst and the vinyl end-capping agent are added into the reaction kettle to react to obtain the first mixed material.
[0017] Specifically, the temperature is first raised to 50-120° C. to allow the dimethylsiloxane ring body to have a certain temperature, and then an alkaline catalyst is added. The temperature of the dimethylsiloxane ring body can be used to dissolve the alkaline catalyst well, making the mixing more uniform and facilitating the homogeneous reaction.
[0018] In some embodiments of the present invention, the reaction time of step S2 is 1.5 to 8 hours.
[0019] In some embodiments of the present invention, in step S2, the weight parts of the dimethylsiloxane ring body is 2000-2500, and the weight parts of the vinyl end-capping agent is 4-20.
[0020] In some embodiments of the present invention, the vinyl end-capping agent includes at least one of vinyl double end-capping agent, vinyl cyclosiloxane, and tetramethyl divinyl siloxane.
[0021] In some preferred embodiments of the present invention, the vinyl end-capping agent is selected from vinyl double end-capping agents.
[0022] In some embodiments of the present invention, step S3 adds 0.5 to 5 parts by weight of the silanol controller to the first mixed material.
[0023] In some embodiments of the present invention, the silanol control agent is selected from at least one of hexamethyldisilazane, vinyl polysilazane, diethylamine, triethylamine, and heptamethyldisilazane.
[0024] In some embodiments of the present invention, the method of removing the alkaline catalyst in step S4 comprises the following steps: raising the temperature to 130-200° C. for 2-6 hours to remove the alkaline catalyst.
[0025] In some embodiments of the present invention, the drying and dehydrating gas in step S4 is selected from at least one of dry nitrogen, dry air, and dry inert gas.
[0026] In some embodiments of the present invention, in step S4, the vacuum degree of the vacuum condition is > -0.05~-0.10MPa, the temperature of the desiccation is 120~200°C, and the time is 2~10h.
[0027] In some embodiments of the present invention, step S4 further comprises a cooling step before the filtration.
[0028] According to a second aspect of the present invention, a vinyl silicone oil prepared according to the above preparation method is provided.
[0029] According to a third aspect of the present invention, a thermally conductive silicone gel is provided, comprising the above-mentioned vinyl silicone oil.
[0030] Specifically, the vinyl silicone oil has a low volatile cyclosiloxane oligomer content (≤0.5%) and a low silanol value. The thermal conductive silicone gel prepared using the vinyl silicone oil as a raw material has a significantly improved oil separation rate, and the emission of pollutants during the vulcanization process is also significantly controlled, which can ensure the safety and environmental protection of the use process. DETAILED DESCRIPTION
[0031] The following will clearly and completely describe the concept of the present invention and the technical effects produced in combination with the embodiments, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by technicians in this field without creative work are all within the scope of protection of the present invention. The test methods used in the embodiments are all conventional methods unless otherwise specified; the materials, reagents, etc. used, unless otherwise specified, can all be reagents and materials obtained from commercial channels. Example
[0032] In this example, vinyl silicone oil 1 was prepared, and the specific process was as follows: (1) The temperature was controlled at ≤90°C, and vacuum (-0.045 MPa) dehydration was performed. Then, 1 part by weight of D3 (dimethylsiloxane ring) and 0.1 part by weight of ethylamine (alkaline compound) were mixed and reacted at 60°C for 6 hours to obtain an alkaline catalyst.
[0033] (2) Add 2000 parts by weight of D3 (dimethylsiloxane ring body) into the reaction kettle and raise the temperature to 50°C; add the alkaline catalyst prepared in step (1) and 4 parts by weight of vinyl double head (vinyl end-capping agent) into the reaction kettle and balance the reaction for 8 hours to obtain a first mixed material.
[0034] (3) Add 0.5 parts by weight of hexamethyldisilazane (silanol control agent) to the first mixed material obtained in step (2), and carry out equilibrium reaction for 0.5 h to obtain a second mixed material.
[0035] (4) The temperature is raised to 130-200°C for 2 hours to remove the alkaline catalyst; then, under the protection of dry and dehydrated nitrogen, the temperature is controlled at 120°C and the vacuum degree is -0.95 MPa for 10 hours, and the mixture is cooled and filtered to obtain vinyl silicone oil 1.
[0036] The viscosity of vinyl silicone oil 1 was measured to be 2200 mPa·s, and the mass percentage of vinyl was 0.223%. Example
[0037] This example prepares a vinyl silicone oil 2, and the specific process is as follows: (1) The temperature was controlled at ≤90°C, and vacuum (-0.095 MPa) dehydration was performed. Then, 10 parts by weight of D4 (dimethylsiloxane ring) and 1.0 parts by weight of triethylamine (alkaline compound) were mixed and reacted at 120°C for 2 hours to obtain an alkaline catalyst.
[0038] (2) Add 2500 parts by weight of D5 (dimethylsiloxane ring body) into the reaction kettle and raise the temperature to 120° C.; add the alkaline catalyst prepared in step (1) and 20 parts by weight of vinyl cyclosiloxane (vinyl end-capping agent) into the reaction kettle and carry out equilibrium reaction for 1.5 hours to obtain a first mixed material.
[0039] (3) Add 5 parts by weight of vinyl polysilazane (silanol control agent) to the first mixed material obtained in step (2), and carry out equilibrium reaction for 6 hours to obtain a second mixed material.
[0040] (4) The temperature is raised to 130-200°C for 6 hours to remove the alkaline catalyst; then, under the protection of dry and dehydrated air, the temperature is controlled at 200°C and the vacuum degree is -0.98 MPa for 4 hours, and the mixture is cooled and filtered to obtain vinyl silicone oil 2.
[0041] The viscosity of vinyl silicone oil 2 was measured to be 2210 mPa·s, and the mass percentage of vinyl was 0.210%. Example
[0042] In this example, vinyl silicone oil 3 was prepared, and the specific process was as follows: (1) The temperature was controlled at ≤90°C, and vacuum (-0.065 MPa) dehydration was performed. Then, 5 parts by weight of D5 (dimethylsiloxane ring) and 0.5 parts by weight of tetramethylammonium hydroxide (alkaline compound) were mixed and reacted at 100°C for 4 hours to obtain an alkaline catalyst.
[0043] (2) Add 2300 parts by weight of D6 (dimethylsiloxane ring body) into the reaction kettle and raise the temperature to 80°C; add the alkaline catalyst prepared in step (1) and 10 parts by weight of tetramethyldivinylsiloxane (vinyl end-capping agent) into the reaction kettle and carry out equilibrium reaction for 5 hours to obtain a first mixed material.
[0044] (3) Add 3 parts by weight of heptamethyldisilazane (silanol control agent) to the first mixed material obtained in step (2), and carry out equilibrium reaction for 3 hours to obtain a second mixed material.
[0045] (4) The temperature was raised to 130-200°C for 4 hours to remove the alkaline catalyst; then, under the protection of argon for drying and dehydration, the temperature was controlled at 150°C and the vacuum degree was -0.96 MPa for 6 hours, and the mixture was cooled and filtered to obtain vinyl silicone oil 3.
[0046] The viscosity of vinyl silicone oil 3 was measured to be 2300 mPa·s, and the mass percentage of vinyl was 0.213%.
[0047] Comparative Example 1 This comparative example prepares vinyl silicone oil a, which differs from Example 1 in that no silanol control agent is added to this comparative example. The specific process is as follows: (1) The temperature was controlled at ≤90°C, and vacuum (-0.045 MPa) dehydration was performed. Then, 1 part by weight of D3 (dimethylsiloxane ring) and 0.1 part by weight of ethylamine (alkaline compound) were mixed and reacted at 60°C for 6 hours to obtain an alkaline catalyst.
[0048] (2) Add 2000 parts by weight of D3 (dimethylsiloxane ring) into a reaction kettle and raise the temperature to 50° C.; add the alkaline catalyst prepared in step (1) and 4 parts by weight of vinyl double capping agent (vinyl end-capping agent) into the reaction kettle and carry out equilibrium reaction for 8 hours to obtain a mixed material.
[0049] (3) The temperature is raised to 130-200°C for 2 hours to remove the alkaline catalyst; then, under the protection of dry and dehydrated nitrogen, the temperature is controlled at 120°C and the vacuum degree is -0.95 MPa for 10 hours, and the mixture is cooled and filtered to obtain vinyl silicone oil a.
[0050] Comparative Example 2 This example prepares vinyl silicone oil b. The difference from Example 2 is that this comparative example is not carried out under vacuum dehydration conditions when preparing the alkaline catalyst, and the dehydration is not carried out under dry dehydration gas protection and vacuum degree of -0.98MPa. The specific process is: (1) 10 parts by weight of D4 (dimethylsiloxane ring) and 1.0 parts by weight of triethylamine (alkaline compound) were mixed and reacted at 120° C. for 2 h to prepare an alkaline catalyst.
[0051] (2) Add 2500 parts by weight of D5 (dimethylsiloxane ring body) into the reaction kettle and raise the temperature to 120° C.; add the alkaline catalyst prepared in step (1) and 20 parts by weight of vinyl cyclosiloxane (vinyl end-capping agent) into the reaction kettle and carry out equilibrium reaction for 1.5 hours to obtain a first mixed material.
[0052] (3) Add 5 parts by weight of vinyl polysilazane (silanol control agent) to the first mixed material obtained in step (2), and carry out equilibrium reaction for 6 hours to obtain a second mixed material.
[0053] (4) Raise the temperature to 130-200°C for 6 hours to remove the alkaline catalyst; then control the temperature at 200°C for 2 hours, cool and filter to obtain vinyl silicone oil b.
[0054] Comparative Example 3 This comparative example prepared vinyl silicone oil c. The difference from Example 3 is that this comparative example did not add a silanol control agent, the preparation of the alkaline catalyst was not carried out under vacuum conditions, and the dehydration was not carried out under dry dehydration gas protection and a vacuum degree of -0.96 MPa. The specific process is: (1) 5 parts by weight of D5 (dimethylsiloxane ring) and 0.5 parts by weight of tetramethylammonium hydroxide (alkaline compound) were mixed and reacted at 100° C. for 4 h to prepare an alkaline catalyst.
[0055] (2) Add 2300 parts by weight of D6 (dimethylsiloxane ring) into a reaction kettle and raise the temperature to 80°C; add the alkaline catalyst prepared in step (1) and 10 parts by weight of tetramethyldivinylsiloxane (vinyl end-capping agent) into the reaction kettle and carry out equilibrium reaction for 5 hours to obtain a mixed material.
[0056] (3) Raise the temperature to 130-200°C for 4 hours to remove the alkaline catalyst; then control the temperature at 150°C for 6 hours, cool and filter to obtain vinyl silicone oil c.
[0057] Test example The yields of the vinyl silicone oils prepared in Examples 1 to 3 and Comparative Examples 1 to 3 and the contents of volatile cyclosiloxane oligomers were measured. The results are shown in Table 1.
[0058] Table 1
[0059] Table 1 shows that the yields of vinyl silicone oils 1 to 3 prepared in Examples 1 to 3 are relatively high, wherein the content of volatile cyclosiloxane oligomers is ≤0.5%, and the silanol values are relatively low. However, in the vinyl silicone oils a to c prepared in Comparative Examples 1 to 3, whether no silanol control agent is added, or the preparation of the alkaline catalyst is not carried out under vacuum dehydration conditions, and the dehydration is not carried out under the protection of dry dehydrating gas, or neither of the above two conditions, the yields of the prepared vinyl silicone oils are relatively low, wherein the content of volatile cyclosiloxane oligomers is >0.5%, and the silanol values are relatively high.
[0060] Therefore, in order to prepare vinyl silicone oil with low volatile cyclosiloxane oligomer content and low silanol value, the above three conditions (addition of silanol control agent; preparation of alkaline catalyst under vacuum dehydration conditions; dehydration under dry dehydrating gas protection and vacuum conditions) are indispensable.
[0061] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A method for preparing vinyl silicone oil, characterized in that: The following steps are involved: S1: Under vacuum dehydration conditions, dimethylsiloxane ring body and alkaline compound are mixed and reacted to prepare an alkaline catalyst; S2: mixing the dimethylsiloxane ring body, the alkaline catalyst and the vinyl end-capping agent, and reacting to obtain a first mixed material; S3: adding a silanol control agent to the first mixed material, and carrying out a balanced reaction for 0.5 to 6 hours to obtain a second mixed material; S4: removing the alkaline catalyst; Then, the product is dehydrated under the protection of a drying and dehydrating gas and vacuum conditions, and the vinyl silicone oil is obtained after filtration.
2. The preparation method according to claim 1, characterized in that: In the vacuum dehydration conditions of step S1, the vacuum degree is -0.045~-0.095MPa, and the temperature of vacuum dehydration is ≤90°C; Preferably, in step S1, 1 to 10 parts by weight of the dimethylsiloxane ring and 0.1 to 1.0 parts by weight of the alkaline compound are mixed and reacted.
3. The preparation method according to claim 1, characterized in that: The dimethylsiloxane ring body includes at least one of a hexamethyltrisiloxane ring body, an octamethylcyclotetrasiloxane ring body, a decamethylpentasiloxane ring body, a dodecamethylcyclohexasiloxane, and a tetradecamethylcycloheptasiloxane; Preferably, the alkaline compound includes at least one of ethylamine, triethylamine, tetramethylammonium hydroxide and ethanolamine.
4. The preparation method according to claim 1, characterized in that: Step S2: firstly add the dimethylsiloxane ring body into a reaction kettle, and heat it to 50-120° C.; then add the alkaline catalyst and the vinyl end-capping agent into the reaction kettle, and react to obtain the first mixed material; Preferably, in step S2, the weight parts of the dimethylsiloxane ring body are 2000-2500, and the weight parts of the vinyl end-capping agent are 4-20; Preferably, the vinyl end-capping agent includes at least one of vinyl double end-capping agent, vinyl cyclosiloxane, and tetramethyl divinyl siloxane.
5. The preparation method according to claim 1, characterized in that: Step S3: adding 0.5 to 5 parts by weight of the silanol control agent to the first mixed material.
6. The preparation method according to claim 1, characterized in that: The silanol control agent is selected from at least one of hexamethyldisilazane, vinyl polysilazane, diethylamine, triethylamine, and heptamethyldisilazane.
7. The preparation method according to claim 1, characterized in that: Step S4: The method for removing the alkaline catalyst comprises the following steps: raising the temperature to 130-200° C. for 2-6 hours to remove the alkaline catalyst.
8. The preparation method according to claim 1, characterized in that: The drying and dehydrating gas in step S4 is selected from at least one of dry nitrogen, dry air, and dry inert gas; Preferably, in step S4, the vacuum degree of the vacuum condition is > -0.05~-0.10MPa, the temperature of the degassing is 120~200°C, and the time is 2~10h.
9. Vinyl silicone oil prepared according to the preparation method according to any one of claims 1 to 8.
10. A thermally conductive silicone gel, characterized in that: The thermally conductive silicone gel comprises the vinyl silicone oil according to claim 9.