Hyperbranched photosensitive resin with photo-initiation group and LDI solder resist ink thereof

By using AB2 type hyperbranched polyester resin and carboxyl modified hyperbranched macromolecular polymer, a hyperbranched photosensitive resin with photoinitiation groups was prepared, which solved the problem of photocuring efficiency and sensitivity loss of LDI solder resist inks, and achieved the High resolution and low defect rate LDI soldering ink improves process efficiency and product performance.

CN118994618APending Publication Date: 2024-11-22SHENZHEN BAILIHE NEW MATERIAL DEV CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411132662.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing LDI soldering inks have losses in terms of photocuring efficiency and sensitivity, and cannot avoid defects caused by molecular entanglement, and cannot meet the requirements of high resolution and low defect rate of laminated circuits.

Method used

AB2 type second-generation or above hyperbranched polyester resin is used as a skeleton, and hyperbranched macromolecular polymers modified by epoxy acrylate end capping and carboxy group were prepared to prepare a hyperbranched photosensitive resin with photoinitiation groups, and combined with A/ The LDI solder-resistant ink composed of component B uses the unique structure of hyperbranched polymer to improve photocuring efficiency and resolution.

Benefits of technology

The three-dimensional spherical structure and tangle-free properties of hyperbranched polymers improve the photocuring speed and resolution, reduce solvent use, reduce process costs, enhance adhesion and scratch resistance, and overcome the dissolution of small-molecular photoinitiators. and poor dispersion problems, improving the photoinduced efficiency and hardness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994618A_ABST
    Figure CN118994618A_ABST
Patent Text Reader

Abstract

The invention discloses hyperbranched photosensitive resin with a photo-initiation group and LDI solder resist ink of the hyperbranched photosensitive resin, and belongs to the technical field of photosensitive materials. The hyperbranched photosensitive resin is a hyperbranched macromolecular polymer (HBAPI) which takes AB2 type hyperbranched polyester resin (HBPE-nG, n is greater than or equal to 2) of more than two generations as a framework, is terminated by epoxy acrylate (HBMA), is modified by carboxyl and is grafted with a photo-initiation group; the alkali-soluble LDI solder resist ink prepared from the hyperbranched photosensitive resin disclosed by the invention has the advantages of small viscosity, high sensitivity, high resolution, high adhesive force, small shrinkage rate, small buckling deformation and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hyperbranched photosensitive resin with a photoinitiating group and an LDI solder resist ink thereof, belonging to the technical field of photosensitive materials. Background Art

[0002] With the rapid development of portable and lightweight electronic products, the high frequency, digitalization and integration of electronic circuits have also made great progress. The traditional film contact and point light source emission mask exposure pattern transfer technology can no longer meet the requirements of high resolution and low defect rate of laminated circuits. Compared with the traditional ink screen printing and film imaging process, the LDI (laser direct imaging) process is much simpler, which can simplify the process and avoid the defects of traditional screen printing and roller printing such as cracks and scratches. In addition, because the film manufacturing process is eliminated, a series of defects generated in the film imaging process are avoided, such as film dimensional stability, film contamination and damage, poor alignment, inconsistent exposure quality and unacceptable line width control, etc. Domestic research on LDI solder resist ink is relatively late, and related patents are very limited. Chinese patent CN113980510A discloses a LDI high-sensitivity solder resist matte black ink and its preparation method. Its main components include: soluble high-sensitivity photocurable resin 45-60%, photoinitiator 1.2-3.5%, photosensitive monomer 10-15%. Its embodiment meets the sensitivity of LDI exposure scale 10 level 500mJ / cm 2 ; Chinese patent CN112965338B discloses a composition and manufacturing method of epoxy acrylic resin for LDI solder resist ink, the resin is composed of biscyclopentadienyloxyethyl acrylate and polyurethane modified epoxy acrylic resin; Chinese patent CN109575675B discloses a solder resist LDI special ink, which includes glossy ink and matte ink, the glossy ink includes a first main agent and a first hardener, and the matte ink includes a second main agent and a second hardener. The glossy ink and the matte ink are evenly stirred to obtain a solder resist LDI special ink, which can solve the problem that the color of the ink surface after direct exposure and development by LDI is lighter than the original matte ink and discolored. The film-forming resin used in the above patents still uses the linear epoxy resin and / or acrylic resin used in traditional solder resist ink, so it is impossible to avoid the loss of photocuring efficiency due to molecular entanglement and the sensitivity loss caused by macromolecular steric hindrance. Summary of the invention

[0003] In order to make up for the shortcomings of the existing LDI solder mask ink, the present invention provides the following technical solutions:

[0004] A hyperbranched photosensitive resin with a photoinitiating group and an LDI solder resist ink thereof, wherein the hyperbranched photosensitive resin is AB 2A hyperbranched macromolecular polymer (HBAPI) with a second generation or higher hyperbranched polyester resin (HBPE-nG, n≥2) as the skeleton, end-capped with epoxy acrylate (HBMA), and then modified with carboxyl groups;

[0005] Preferably, the hyperbranched photosensitive resin is HBAPI with second-generation HBPE-2G and third-generation HBPE-3G as the skeleton.

[0006] Preferably, the method for preparing the hyperbranched photosensitive resin comprises the following four steps:

[0007] (1) Pentaerythritol (PER), 2,2-dihydroxymethylpropionic acid (BMPA) and p-toluenesulfonic acid (PTSA) are added to a three-necked flask equipped with a stirring paddle, a nitrogen inlet and a drying tube, wherein the molar ratio of BMPA to PER is 12:1 and the addition ratio of PTSA is 0.5% of the mass of BMPA; the temperature is raised to 120-170° C. under mechanical stirring and nitrogen flow, and after reacting and removing water for 1-4 hours, the nitrogen is turned off and vacuum is drawn, and the reaction is continued for 1-4 hours, and then the pressure is restored to normal pressure to obtain a second-generation hyperbranched polyester (HBPE-2G), the synthesis principle and typical molecular structure of which are shown in formula (I).

[0008]

[0009] Continue to add BMPA and PTSA, the second addition ratio of PTSA is 0.5% of the mass of BMPA added for the second time; the mixture is reacted at 120-170° C. for 1-4 hours under nitrogen protection, then the nitrogen is turned off and vacuumized, and the reaction is continued for 1-4 hours before stopping the reaction to obtain a second-generation or higher hyperbranched polyester (HBPE-nG, n>2);

[0010] Preferably, the reaction temperature is 130° C. to 150° C., and the reaction time for each step is 2 hours.

[0011] (2) Put polycarboxylic acid anhydride (AH) and solvent into a three-necked flask with a stirring paddle, a nitrogen inlet and a drying tube, the weight ratio of AH to solvent is 1:0.5-1:2, after AH is dissolved, put into the second generation or more hyperbranched polyester (HBPE-nG, n≥2) prepared in the previous step, the molar ratio of AH to hydroxyl groups in HBPE is 1:1, and react at 80°C-120°C for 4-12 hours to obtain a hyperbranched polymer (HBAH) with terminal carboxyl groups. The synthesis principle and the typical molecular structure of HBHA with HBPE-2G as the skeleton are shown in formula (II):

[0012]

[0013] Preferably, the polycarboxylic anhydride is selected from at least one of maleic anhydride (MAH), succinic anhydride (SAH), phthalic anhydride (PAH), tetrahydrophthalic anhydride (THPA), hexahydrophthalic anhydride (HHPA), methylhexahydrophthalic anhydride (MHHPA), trimellitic anhydride (TMA), nadic anhydride (NAH), methyl nadic anhydride (MNAH) and hydrogenated methyl nadic anhydride (HMNAH), and more preferably succinic anhydride (SAH), tetrahydrophthalic anhydride (THPA) and hexahydrophthalic anhydride (HHPA);

[0014] Preferably, the solvent is selected from at least one of dipropylene glycol methyl ether (DPM), dibasic acid ester (DBE), toluene (TL), xylene (XY), trimethylbenzene (TYL), acetone (CP), butanone (MEK), cyclohexanone (CYC), dioxane (DIOX), tetrahydrofuran (THF), diacetone alcohol (DAA), and dimethylformamide (DMF), and DPM, DBE, XY, and TYL are more preferred;

[0015] Preferably, the reaction temperature is 100° C. to 110° C., and the reaction time is 5 to 7 hours.

[0016] (3) The carboxyl-terminated hyperbranched polymer (HBAH) obtained in the previous step and glycidyl methacrylate (GMA) are placed in a three-necked flask equipped with a stirring paddle, a nitrogen inlet and a drying tube, the molar ratio of GMA to carboxylic acid being 1:1, and appropriate amounts of catalyst and inhibitor are added dropwise. The reaction is carried out at 80° C. to 120° C. for 4 to 12 hours. The reaction is stopped when the acid value is less than 5 mgKOH / Kg to obtain an epoxy acrylate-terminated hyperbranched polymer (HBMA). The synthesis principle and the typical molecular structure with HBPE-2G as the skeleton are shown in formula (III):

[0017]

[0018] Preferably, the catalyst is selected from at least one of N,N-dimethylbenzylamine (DMBA), tetramethylammonium bromide (TMAB), tetraethylammonium bromide (TEAB), tetrabutylammonium bromide (TBAB), triethanolamine (TEAA), triphenylphosphine (TPP), and chromium acetylacetonate (CrA), and more preferably triphenylphosphine (TPP) and tetraethylammonium bromide (TEAB);

[0019] Preferably, the inhibitor is selected from at least one of hydroquinone (HQ), 2,6-di-tert-butyl-p-cresol (BHT), and p-hydroxyanisole (MEHQ); p-hydroxyanisole (MEHQ) is further preferred;

[0020] Preferably, the reaction temperature is 100° C. to 110° C., the reaction time is 6 to 9 hours, and the reaction is stopped when the acid value is less than 3 mgKOH / Kg.

[0021] (4) A polycarboxylic acid anhydride (AH), a reactive photoinitiator (PI) and a solvent are added to a three-necked flask with a stirring paddle, a nitrogen inlet and a drying tube, wherein the weight ratio of AH to the solvent is 1:0.5 to 1:2. After AH and PI are dissolved, the epoxy acrylate-terminated hyperbranched polymer (HBMA) prepared in the previous step is added, wherein the molar ratio of the hydroxyl groups in AH and HBMA is 0.2:1 to 1:1. The reaction is carried out at 80° C. to 120° C. for 4 to 12 hours. When the acid value becomes constant, the reaction is stopped to obtain a carboxyl-modified epoxy acrylate-terminated hyperbranched photosensitive resin (HBAPI) with a photoinitiator group. The synthesis principle and the typical molecular structure with HBPE-2G as the skeleton are shown in formula (IV):

[0022]

[0023] Preferably, the X group is selected from at least one of formula (V):

[0024]

[0025] Preferably, the Y group is selected from at least one of the formula (VI):

[0026]

[0027] Preferably, the polycarboxylic anhydride is selected from at least one of maleic anhydride (MAH), succinic anhydride (SAH), phthalic anhydride (PAH), tetrahydrophthalic anhydride (THPA), hexahydrophthalic anhydride (HHPA), methylhexahydrophthalic anhydride (MHHPA), trimellitic anhydride (TMA), nadic anhydride (NAH), methyl nadic anhydride (MNAH) and hydrogenated methyl nadic anhydride (HMNAH), and more preferably tetrahydrophthalic anhydride (THPA) and hexahydrophthalic anhydride (HHPA);

[0028] Preferably, the solvent is selected from at least one of dipropylene glycol methyl ether (DPM), dibasic acid ester (DBE), toluene (TL), xylene (XY), trimethylbenzene (TYL), acetone (CP), butanone (MEK), cyclohexanone (CYC), dioxane (DIOX), tetrahydrofuran (THF), diacetone alcohol (DAA), and dimethylformamide (DMF), and DPM, DBE, XY, and TYL are more preferred;

[0029] Preferably, the molar ratio of AH to the hydroxyl group in HBMA is in the range of 0.5:1 to 0.7:1, and the reaction is carried out at 100°C to 110°C for 5 to 7 hours. Preferably, the reactive photoinitiator (PI) comprises a reactive main initiator and a reactive co-initiator; the reactive main initiator is selected from at least one of formula (VII):

[0030]

[0031] Preferably, the reactive co-initiator is selected from at least one of formula (VIII):

[0032]

[0033] Preferably, the LDI solder resist ink based on the hyperbranched photosensitive resin is composed of A / B components, and the weight ratio of A / B components is 8:2-7:3; component A comprises 40-80wt% of the hyperbranched photosensitive resin obtained according to the above preparation method, 1-10wt% of the diluent, 10-40wt% of the filler and 0.1-5wt% of the functional additive;

[0034] Component B comprises 20-60wt% epoxy resin, 10-20wt% active monomer, 5-20wt% diluent, 10-30wt% curing agent, 20-40wt% filler and 0.1-5wt% functional additive;

[0035] Preferably, the reactive diluent includes but is not limited to: trimethylolpropane triacrylate (TMPTA), pentaerythritol triacrylate (PETA), pentaerythritol tetraacrylate (PETA4), dipentaerythritol hexaacrylate (DPHA), isobornyl acrylate (IBOA), isobornyl methacrylate (IBOMA), hexanediol diacrylate (HDDA), 1,6-hexanediol diacrylate (HDDA), polyethylene glycol diacrylate (PEGDA), dipropylene glycol diacrylate (DPGDA), tripropylene glycol diacrylate (TPGDA); further preferably trimethylolpropane triacrylate (TMPTA), pentaerythritol tetraacrylate (PETA4), dipentaerythritol hexaacrylate (DPHA); preferably, the epoxy resin includes but is not limited to: at least one of bisphenol A epoxy resin, novolac epoxy resin, biphenyl epoxy resin, naphthalene epoxy resin, anthracene epoxy resin, phenoxy epoxy resin, preferably o-cresol epoxy resin, biphenyl epoxy resin;

[0036] Preferably, the curing agent includes but is not limited to: at least one of dicyandiamide (DIC), imidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, succinic acid hydrazide, adipic acid dihydrazide, sebacic acid hydrazide, isophthalic acid hydrazide, p-hydroxybenzoic acid hydrazide (POBH), diaminomaleonitrile and its derivatives, diaminodiphenyl sulfone (DDS), diaminodiphenylmethane (DDM), metaphenylenediamine (m-PDA) and benzoxazine, and dicyandiamide (DIC) and imidazole are more preferred;

[0037] Preferably, the filler includes but is not limited to: SiO 2 、TiO2 、ZrO 2 、ZnO、MgO、CaO、Al 2 O 3 , K 2 CO 3 ,BaSO 4 、CaCO 3 , talc, montmorillonite, zeolite, mica powder, graphene, fullerene, carbon nanotubes, more preferably SiO 2 、TiO 2 ,BaSO 4 , talc, montmorillonite;

[0038] Preferably, the auxiliary agents include but are not limited to: defoaming agent, leveling agent, rheological agent, curing agent, coupling agent, pigment, dye, antioxidant, ultraviolet light absorber, etc., which can be selected according to general technology.

[0039] Beneficial effects:

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] (1) Hyperbranched polymers have a unique three-dimensional spherical molecular structure with no entanglement between molecules. Their viscosity is much lower than that of linear oligomers of the same molecular weight, which can reduce the use of solvents and reduce negative impacts on the environment.

[0042] (2) The end-capped photosensitive groups of the hyperbranched polymer are aggregated on the surface of the spherical molecules, and the curing speed is much faster than that of linear oligomers with similar molecular weight, which can shorten the process cycle and reduce the process cost;

[0043] (3) When the photoresist prepared with highly branched polymers is developed after exposure, the image is clear and the cross-section is good, so a higher resolution can be obtained because there is no entanglement between the uncross-linked molecules;

[0044] (4) Highly branched polymers have dense branch structures, and the proportion of active diluents is small or even unsuitable. Therefore, the shrinkage rate during curing is very small, which is conducive to improving adhesion, maintaining dimensional stability, and avoiding defects such as warping, deformation, and cracking;

[0045] (5) Hyperbranched polymers have active groups on their side chains and nanopores exist between the side chains, so they have good compatibility with inorganic nanoparticles, which can further reduce shrinkage and increase surface hardness and scratch resistance;

[0046] (6) The hyperbranched system has a high crosslinking density after curing, and has high hardness, high wear resistance and solvent resistance;

[0047] (7) The photoinitiator groups grafted onto the hyperbranched macromolecules are aggregated on the surface of the spherical molecules, overcoming the defects of poor solubility and dispersion of small molecule photoinitiators in the resin, and the photoinitiator speed is greatly improved;

[0048] (8) The two photoinitiator groups have a synergistic effect, increasing the photoinitiator efficiency;

[0049] (9) It overcomes a series of shortcomings caused by small molecule initiators, such as yellowing, odor, and toxicity. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 Exposure test photos of Examples 1 to 5 and the reference example DETAILED DESCRIPTION

[0051] The present invention is further explained below in conjunction with specific embodiments. For process parameters not particularly noted, conventional techniques may be used.

[0052] Example 1

[0053] The hyperbranched photosensitive resin with photoinitiator groups is synthesized by the following four steps:

[0054] Step 1: Preparation of second generation hyperbranched polyester (HBPE-2G):

[0055] In a three-necked flask equipped with a magnetic stirrer, a thermometer, a condenser, and a nitrogen tube, 87 mmol (11.9 g) of pentaerythritol (PER), 1.044 mol (140 g) of 2,2-dihydroxymethylpropionic acid (BMPA), and 7 g of p-toluenesulfonic acid were added.

[0056] (PTSA); the oil bath was heated to 140°C, and the mixture was reacted under nitrogen protection to remove the water formed during the reaction; after reacting for 2 hours, the nitrogen was turned off, the flask was sealed and connected to a vacuum line (1.2 KPa), and the pressure was restored to normal pressure in 1 hour; the second-generation hyperbranched polyester (HBPE-2G) was obtained, and the measured yield was 88.1%;

[0057] Step 2: Preparation of the second generation hyperbranched polymer (HBAH) with carboxyl groups at the end:

[0058] 1.12 mol (170.4 g) of tetrahydrophthalic anhydride (THPA), 70 g of dibasic acid ester (DBE) and 70 g of xylene (XY) were put into a three-necked flask with a stirring paddle, a nitrogen inlet and a drying tube. After THPA was completely dissolved, 113 g of the second-generation hyperbranched polyester (HBPE-2G) prepared in the previous step was added, and the mixture was reacted at 110° C. for 6 hours to obtain a hyperbranched polymer (HBAH) with a carboxyl terminal group, and the measured yield was 97.6%;

[0059] Step 3: Preparation of epoxy acrylate terminated hyperbranched polymer (HBMA):

[0060] 370 g of the carboxyl-terminated hyperbranched polymer (HBAH) obtained in the previous step and 992 mmol (141 g) of glycidyl methacrylate (GMA) were put into a three-necked flask with a stirring blade, a nitrogen inlet and a drying tube, 2 g of triphenylphosphine (TPP) and 0.4 g of p-hydroxyanisole (MEHQ) were added dropwise, and the mixture was reacted at 110° C. for 6 hours. The acid value was measured by automatic potentiometric titration to be 2.4 mgKOH / Kg, and an epoxy acrylate-terminated hyperbranched polymer (HBMA) was obtained, with a measured yield of 96.8%;

[0061] Step 4: Preparation of the second generation hyperbranched photosensitive resin (HBAPI) grafted with a photoinitiator and capped with carboxyl-modified epoxy acrylate:

[0062] 110 mmol (16.8 g) of tetrahydrophthalic anhydride (THPA), 8.3 g of thioxanthone-1-carboxylic acid having a molecular structure as shown in formula (IX), 1.6 g of p-dimethylaminobenzoic acid having a molecular structure as shown in formula (X), 12 g of dibasic acid ester (DBE) and 8 g of xylene (XY) are put into a three-necked flask with a stirring paddle, a nitrogen inlet and a drying tube. After THPA and PI are completely dissolved, 83 g of the epoxy acrylate-terminated hyperbranched polymer (HBMA) prepared in the previous step is added, and the mixture is reacted at 110° C. for 7 hours. The acid value is measured by automatic potentiometric titration to be 52.6 mgKOH / Kg, and a hyperbranched photosensitive resin (HBAPI-1) with a photoinitiator group and carboxyl-modified epoxy acrylate-terminated is obtained. The actual yield is 95.7%, and the chemical structure thereof is shown in formula (XI);

[0063]

[0064] Example 2

[0065] 110mmol (16.8g) of tetrahydrophthalic anhydride (THPA), 8.6g of thioxanthone-1-carboxylic acid, 1.3g of 1-carboxypropylpiperidine, 12g of dibasic acid ester (DBE) and 8g of xylene (XY) were put into a three-necked flask with a stirring paddle, a nitrogen inlet and a drying tube, and after THPA and PI were completely dissolved, 83g of the epoxy acrylate-terminated hyperbranched polymer (HBMA) obtained in Example 1 was added, and the reaction was carried out at 110°C for 7 hours. The acid value was measured by automatic potentiometric titration to be 51.7mgKOH / Kg, and a hyperbranched photosensitive resin (HBAPI-2) with a photoinitiator group and carboxyl-modified epoxy acrylate-terminated was obtained. The measured yield was 96.2%, and its chemical structure is shown in Formula (XII);

[0066]

[0067] Example 3

[0068] 110 mmol (16.8 g) of tetrahydrophthalic anhydride (THPA), 5.3 g of thioxanthone-1-carboxylic acid, 3.4 g of (4-carboxymethyl 2,6-dimethylbenzoyl) diphenylphosphine oxide, 1.1 g of 1-carboxypropylpiperidine, 12 g of dibasic acid ester (DBE) and 8 g of xylene (XY) were put into a three-necked flask with a stirring paddle, a nitrogen inlet and a drying tube. After THPA and PI were completely dissolved, 83 g of the epoxy acrylate-terminated hyperbranched polymer (HBMA) obtained in Example 1 was added, and the mixture was reacted at 110° C. for 7 hours. The acid value was measured by automatic potentiometric titration to be 50.8 mgKOH / Kg. A hyperbranched photosensitive resin (HBAPI-3) with a photoinitiator group and carboxyl-modified epoxy acrylate-terminated was obtained. The actual yield was 95.7%, and its chemical structure is shown in Formula (XIII);

[0069]

[0070] Example 4

[0071] 110mmol (16.8g) of tetrahydrophthalic anhydride (THPA), 5.5g of thioxanthone-1-carboxylic acid, 3.2g of 2-carboxymethyl-anthraquinone, 0.7g of 1-carboxypropylpiperidine, 0.8g of p-dimethylaminobenzoic acid, 12g of dibasic acid ester (DBE) and 8g of xylene (XY) were put into a three-necked flask with a stirring blade, a nitrogen inlet and a drying tube, and after THPA and PI were completely dissolved, 83g of the epoxy acrylate-terminated hyperbranched polymer (HBMA) obtained in Example 1 was put into the flask, and the reaction was carried out at 110°C for 7 hours. The acid value was measured by automatic potentiometric titration to be 51.1mgKOH / Kg, and a hyperbranched photosensitive resin (HBAPI-4) with a photoinitiator group and carboxyl-modified epoxy acrylate-terminated was obtained. The actual yield was 97.5%, and its chemical structure is shown in Formula (XIV);

[0072]

[0073] Example 5

[0074] 110 mmol (16.8 g) of tetrahydrophthalic anhydride (THPA), 4.7 g of thioxanthone-1-carboxylic acid, 2.5 g of (4-carboxymethyl 2,6-dimethylbenzoyl) diphenylphosphine oxide, 1.3 g of 2-carboxymethyl-anthraquinone, 1.1 g of 1-carboxypropylpiperidine, 12 g of dibasic acid ester (DBE) and 8 g of xylene (XY) were put into a three-necked flask with a stirring paddle, a nitrogen inlet and a drying tube. After THPA and PI were completely dissolved, 83 g of the epoxy acrylate-terminated hyperbranched polymer prepared in Example 1 was added.

[0075] (HBMA), reacted at 110°C for 7 hours, the acid value was measured by automatic potentiometric titration method to be 50.7 mgKOH / Kg, and a hyperbranched photosensitive resin (HBAPI-5) with photoinitiator groups and carboxyl-modified epoxy acrylate end-capping was obtained, the measured yield was 97.2%, and its chemical structure is shown in Formula (XV);

[0076]

[0077] The hyperbranched photosensitive resins prepared in Examples 1 to 5 were prepared into LDI solder resist ink component A according to the proportions in Table 1, and three-roll milled for 30 min, filtered for 340 T, and then mixed with fixed B component * in a ratio of 3:1, and then stirred at 150 rpm for 20 min to prepare five LDI solder resist inks.

[0078] Table 1

[0079]

[0080]

[0081] * Component B CY90HD04 was provided by Zhaoqing Yueyang Electronic Technology Co., Ltd.

[0082] **The composite additive BLH-AC47 includes color powder, defoaming agent, inhibitor, leveling agent, antioxidant, etc., which is provided by Lianyungang Bailihe.

[0083] Reference example

[0084] The reference example is the LDI solder mask ink YC9001-G41 based on linear epoxy acrylic resin produced by Zhaoqing Chaoyang Electronic Technology Co., Ltd.

[0085] Test Case

[0086] The LDI solder resist ink prepared in the embodiment and the reference example was screen-printed on the PCB, pre-baked at 75°C for 45 minutes, and then directly exposed with a 50W composite laser light source with a spectrum of 365-405nm. Finally, the temperature was 30°C, the pressure was 0.2MPa, and the concentration was 1.0% Na 2 CO 3 Develop in developer for 100 seconds, post-bake at 150°C x 60 minutes, and circulate hot air for curing. The test items and experimental results are shown in Table 2:

[0087] Table 2

[0088]

[0089]

[0090] (1) Soak in 10vol% HCl for 30 minutes (25°C)

[0091] (2) Soak in 10wt% NaOH for 30 min (25°C)

[0092] (3) Soak in isopropyl alcohol for 30 minutes (25°C)

[0093] The test results in Table 2 show that the LDI solder resist ink using the hyperbranched polymer prepared in the present invention as a skeleton has excellent properties such as fast exposure speed, high resolution, and dimensional stability compared to the LDI solder resist ink synthesized with linear epoxy acrylic resin.

[0094] The above description is only a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.

Claims

1. A hyperbranched photosensitive resin with a photoinitiator group and its LDI solder resist ink, characterized in that: The resin is a hyperbranched macromolecular polymer (HBAPI) with an AB2 type second-generation or higher hyperbranched polyester resin (HBPE-nG, n≥2) as the skeleton, epoxy acrylate end-capping (HBMA), carboxyl modification and grafting of photoinitiator groups.

2. The hyperbranched photosensitive resin with a photoinitiator group and the LDI solder resist ink thereof according to claim 1, characterized in that: The preparation of the resin includes the following four steps: (1) Pentaerythritol (PER), 2,2-dihydroxymethylpropionic acid (BMPA) and p-toluenesulfonic acid (PTSA) are added to a three-necked flask equipped with a stirring paddle, a nitrogen inlet and a drying tube, wherein the molar ratio of BMPA to PER is 12:1 and the addition ratio of PTSA is 0.5% of the mass of BMPA; the temperature is raised to 120-170° C. under mechanical stirring and nitrogen flow, and after reacting and removing water for 1-4 hours, the nitrogen is turned off and vacuum is drawn, and the reaction is continued for 1-4 hours, and then the pressure is restored to normal pressure to obtain a second-generation hyperbranched polyester (HBPE-2G), the synthesis principle and typical molecular structure of which are shown in formula (I). Continue to add BMPA and PTSA, the second addition ratio of PTSA is 0.5% of the mass of BMPA added for the second time; the mixture is reacted for 1 to 4 hours under nitrogen protection, then the nitrogen is turned off and vacuumized, and the reaction is continued for 1 to 4 hours and then stopped to obtain a second-generation or higher hyperbranched polyester (HBPE-nG, n>2). (2) A polycarboxylic acid anhydride (AH) and a solvent are added to a three-necked flask equipped with a stirring paddle, a nitrogen inlet and a drying tube, wherein the weight ratio of AH to the solvent is 1:0.5 to 1:

2. After AH is dissolved, the second-generation or higher hyperbranched polyester (HBPE-nG, n≥2) prepared in the previous step is added, wherein the molar ratio of AH to the hydroxyl group in HBPE is 1:

1. The mixture is reacted at 80°C to 120°C for 4 to 12 hours to obtain a carboxyl-terminated hyperbranched polymer (HBAH). The synthesis principle and the typical second-generation hyperbranched molecular structure are shown in formula (II). (3) The carboxyl-terminated hyperbranched polymer (HBAH) obtained in the previous step and glycidyl methacrylate (GMA) are placed in a three-necked flask equipped with a stirring paddle, a nitrogen inlet and a drying tube, the molar ratio of GMA to carboxylic acid being 1:1, and appropriate amounts of catalyst and inhibitor are added dropwise. The reaction is carried out at 80° C. to 120° C. for 4 to 12 hours. The reaction is stopped when the acid value is less than 5 mgKOH / Kg to obtain an epoxy acrylate-terminated hyperbranched polymer (HBMA). The synthesis principle and typical second-generation hyperbranched molecular structure are shown in formula (III). (4) A polycarboxylic acid anhydride (AH), a reactive photoinitiator (PI) and a solvent are placed in a three-necked flask equipped with a stirring paddle, a nitrogen inlet and a drying tube, wherein the weight ratio of AH to the solvent is 1:0.5 to 1:

2. After AH and PI are dissolved, the epoxy acrylate-terminated hyperbranched polymer (HBMA) prepared in the previous step is added, wherein the molar ratio of the hydroxyl groups in AH and HBMA is in the range of 0.2:1 to 1:

1. The reaction is carried out at 80° C. to 120° C. for 4 to 12 hours. When the acid value becomes constant, the reaction is stopped to obtain a hyperbranched photosensitive resin (HBAPI) with a photoinitiator group and carboxyl-modified epoxy acrylate-terminated. The synthesis principle and the typical second-generation hyperbranched molecular structure are shown in formula (IV). Wherein the X group is selected from at least one of formula (V): The Y group is selected from at least one of formula (VI):

3. The polycarboxylic anhydride of claim 2 is at least one selected from the group consisting of maleic anhydride (MAH), succinic anhydride (SAH), phthalic anhydride (PAH), tetrahydrophthalic anhydride (THPA), hexahydrophthalic anhydride (HHPA), methylhexahydrophthalic anhydride (MHHPA), trimellitic anhydride (TMA), nadic anhydride (NAH), methylnadic anhydride (MNA) and hydrogenated methylnadic anhydride (HMNA); The catalyst is selected from at least one of N,N-dimethylbenzylamine (DMBA), tetramethylammonium bromide (TMAB), tetraethylammonium bromide (TEAB), tetrabutylammonium bromide (TBAB), triethanolamine (TEAA), triphenylphosphine (TPP), and chromium acetylacetonate (CrA); The solvent is selected from at least one of dipropylene glycol methyl ether (DPM), dibasic acid ester (DBE), toluene (TL), xylene (XY), trimethylol (TYL), acetone (CP), butanone (MEK), cyclohexanone (CYC), dioxane (DIOX), tetrahydrofuran (THF), diacetone alcohol (DAA), and dimethylformamide (DMF); the inhibitor is selected from at least one of hydroquinone (HQ), 2,6-di-tert-butyl-p-cresol (BHT), and p-hydroxyanisole (MEHQ). The reactive photoinitiator (PI) comprises a reactive main initiator and a reactive co-initiator; the reactive main initiator is selected from at least one of formula (VII): The reactive co-initiator is selected from at least one of formula (VIII):

4. The hyperbranched photosensitive resin with a photoinitiator group and the LDI solder resist ink thereof according to claim 1, characterized in that: The LDI solder resist ink is composed of A / B components, and the weight ratio of the A / B components is 8:2 to 7:3; Component A comprises 40-80 wt% of the hyperbranched photosensitive resin prepared according to claim 2, 5-15 wt% of an active monomer, 0-10 wt% of a diluent, 10-30 wt% of a filler and 0.1-5 wt% of a functional additive; Component B comprises 20-60wt% epoxy resin, 10-20wt% active monomer, 5-20wt% diluent, 10-30wt% curing agent, 20-40wt% filler and 0.1-5wt% functional additive; The active monomers described in claim 4 include but are not limited to: trimethylolpropane triacrylate (TMPTA), pentaerythritol triacrylate (PETA), pentaerythritol tetraacrylate (PETA4), dipentaerythritol hexaacrylate At least one of (DPHA), isobornyl acrylate (IBOA), isobornyl methacrylate (IBOMA), hexanediol diacrylate (HDDA), 1,6-hexanediol diacrylate (HDDA), polyethylene glycol diacrylate (PEGDA), dipropylene glycol diacrylate (DPGDA), and tripropylene glycol diacrylate (TPGDA); the epoxy resin includes but is not limited to: at least one of bisphenol A epoxy resin, novolac epoxy resin, biphenyl epoxy resin, naphthalene epoxy resin, anthracene epoxy resin, and phenoxy epoxy resin; The curing agent includes but is not limited to: at least one of dicyandiamide (DIC), imidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, succinic acid hydrazide, adipic acid dihydrazide, sebacic acid hydrazide, isophthalic acid hydrazide, p-hydroxybenzoic acid hydrazide (POBH), diaminomaleonitrile and its derivatives, diaminodiphenyl sulfone (DDS), diaminodiphenylmethane (DDM), m-phenylenediamine (m-PDA) and benzoxazine; The diluent includes but is not limited to: any one or a mixture of dimethyl succinate, dimethyl glutarate or dimethyl adipate; The filler includes but is not limited to: at least one of SiO2, TiO2, ZrO2, ZnO, MgO, CaO, Al2O3, K2CO3, BaSO4, CaCO3, talc, montmorillonite, zeolite, mica powder, graphene, fullerene, and carbon nanotubes. The auxiliary agents include but are not limited to: defoaming agents, leveling agents, rheological agents, coupling agents, pigments, dyes, antioxidants, ultraviolet light absorbers, etc., which can be selected according to general techniques.

Citation Information

Cited By

  • Ultrathin anti-corrosion film based on electrophoretic deposition and positive photosensitive mechanism and application of ultrathin anti-corrosion film

    CN121028465A

  • Ultra-thin resist film based on electrophoretic deposition and positive photosensitive mechanism and application thereof

    CN121028465B