Fluorescent self-healing injectable hydrogel and preparation method thereof

By combining bioluminescent molecules with N-carboxyethyl chitosan and oxidized sodium alginate, a fluorescent self-healing injectable hydrogel is solved, and the problems of poor biosafety and lack of real-time monitoring functions of fluorescent substances in the prior art are solved. , realizes biocompatibility and self-healing, and expands the application in the field of biomedical science.

CN118994643AActive Publication Date: 2024-11-22SHAANXI UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411093498.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The existing self-healing injectable hydrogels lack the in-situ real-time monitoring function, and the fluorescent substances have poor biosafety and cumbersome preparation technology, making it difficult to effectively apply in the field of biomedical medicine.

Method used

By combining bioluminescent molecules with N-carboxyethyl chitosan and sodium oxidized alginate, a fluorescent self-healing injectable hydrogel is formed, which enhances the fluorescence characteristics using co-doped nitrogen and sulfur carbon dots, and through coupling reactions Cross-linking with dynamic imine bonds to achieve biocompatibility and self-healing.

Benefits of technology

It realizes non-invasive real-time monitoring function, simplifies the preparation process, improves biocompatibility and fluorescence performance, and expands its application prospects in the field of biomedical science.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994643A_ABST
    Figure CN118994643A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of fluorescent self-healing injectable hydrogel. The preparation method comprises the following steps: anchoring biocompatible fluorescent small molecules on a polysaccharide macromolecular chain through EDC / NHS coupling reaction, and then performing in-situ crosslinking through dynamic imine bonds under physiological conditions to prepare the fluorescent self-healing injectable hydrogel. The fluorescent self-healing injectable hydrogel has self-healing property, injectable property, shape adaptability, biodegradability, cytocompatibility, histocompatibility and outstanding fluorescent effect, and can be used for nondestructive, in-situ and real-time detection, so that a new strategy for synthesizing the polysaccharide-based fluorescent self-healing injectable hydrogel under mild conditions is provided; and meanwhile, a new thought for establishing a system model of the in-situ real-time monitoring biomedical platform of the minimally invasive interventional therapy technology is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flexible biomaterials and relates to a fluorescent self-healing injectable hydrogel and a preparation method thereof. Background Art

[0002] Biocompatible self-healing injectable hydrogels have broad application prospects in the biomedical field. Their characteristics are that they can spontaneously restore their structure and function after being damaged, thereby significantly improving their performance as smart flexible materials. As smart multifunctional biomaterials, self-healing injectable hydrogels can be combined with minimally invasive interventional treatment technologies, and are widely used in the fields of tissue engineering, drug / cell delivery, and biosensors. The advantages of self-healing injectable hydrogels are in-situ gelation in the syringe → injection of gel at the target site → autonomous healing of gel particles → remodeling at the target site, which changes the fluid operation method of traditional injectable hydrogels, that is, loading the precursor solution into the syringe → injecting the solution at the target site → gelation at the target site. At the same time, self-healing injectable hydrogels make up for many shortcomings of traditional injectable hydrogels, such as the loss of drugs and cells due to diffusion before gelation, the difficulty in controlling the gelation time, and the potential toxicity of chemical substances (such as monomers, initiators, etc.). Although many advances have been made, conventional self-healing injectable hydrogels still lack the function of in-situ real-time monitoring, and are limited by the difficulty of non-invasive monitoring and tracking after being implanted in the body. To date, non-invasiveness and tracking capabilities in vivo remain urgent issues to be solved for self-healing injectable hydrogels.

[0003] Fluorescence monitoring technology has the advantages of rapid response, high sensitivity, high contrast and non-invasiveness, which facilitates the real-time monitoring of fluorescent hydrogels. Fluorescent hydrogels with good biocompatibility have attracted much attention in the biomedical field and have specific applications in biomedical platforms, such as bioimaging and biomonitoring tracking. Various fluorescent substances (such as lanthanide ions, organic dyes, quantum dots, fluorescent proteins and metal ligands) can be coupled or doped into the hydrogel matrix to give the hydrogel fluorescent properties. However, most fluorescent substances have the disadvantages of biological toxicity, poor water solubility and complicated preparation process, which greatly limits their practical application in the biomedical field.

[0004] Multifunctional fluorescent self-healing injectable hydrogels have great application potential in biomedical platforms for real-time biological imaging monitoring. Although existing strategies focus on the development of various self-healing injectable hydrogels suitable for the biomedical field, few studies have focused on the application of self-healing injectable hydrogels that have fluorescence properties, biocompatibility and biodegradability in the biomedical field. Fluorescent self-healing injectable hydrogels are expected to be monitored by real-time imaging in vivo through non-invasive methods without interfering with the efficacy and safety of treatment. However, how to develop a simple and effective strategy to fix biocompatible fluorescent substances in the dynamic hydrogel three-dimensional network structure and synthesize fluorescent self-healing injectable hydrogels for biomedical platforms has become a major problem that current scientific researchers need to solve urgently.

[0005] Therefore, it is necessary to combine fluorescent substances with excellent biosafety and easy operation with hydrogels to prepare fluorescent self-healing injectable hydrogels that have excellent fluorescence properties and the functions of polysaccharide-based dynamic hydrogels (self-healing, injectability, biocompatibility and biodegradability, etc.), so as to achieve non-invasive monitoring and tracking and minimally invasive interventional treatment. Summary of the invention

[0006] In view of the problems existing in the prior art, the present invention provides a fluorescent self-healing injectable hydrogel and a preparation method thereof, thereby solving the technical problems in the prior art of poor biosafety of fluorescent substances, poor fluorescence effect, and lack of in situ real-time monitoring function of the self-healing injectable hydrogel.

[0007] The present invention is achieved through the following technical solutions:

[0008] A method for preparing a fluorescent self-healing injectable hydrogel comprises the following steps:

[0009] S1: dissolving the bioluminescent molecule in a 2-morphineethanesulfonic acid solution, then adding 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, stirring and dissolving to obtain a mixed solution; adding a 2-morphineethanesulfonic acid solution of N-carboxyethyl chitosan to the mixed solution, stirring and reacting to obtain a bioluminescent molecule / N-carboxyethyl chitosan polymer;

[0010] S2: Mixing the PBS solution containing the bioluminescent molecule / N-carboxyethyl chitosan polymer with the PBS solution containing oxidized sodium alginate to prepare the fluorescent self-healing injectable hydrogel.

[0011] Preferably, the preparation of the bioluminescent molecule is specifically as follows: citric acid powder and cysteine ​​are uniformly mixed, heated for reaction, the product is washed, and then recrystallized to obtain the bioluminescent molecule.

[0012] Preferably, the N-carboxyethyl chitosan is prepared by mixing chitosan and acrylic acid and reacting them; wherein, in the mixed solution of chitosan and acrylic acid, the concentration of chitosan is 5-10 mM, and the concentration of acrylic acid is 20-25 mM.

[0013] Preferably, the deacetylation degree of the chitosan is 86% to 88%, and the molecular weight of the chitosan is 2*10 5 ~3*10 5 g / mol.

[0014] Preferably, the amino substitution degree of the N-carboxyethyl chitosan is 48% to 50%.

[0015] Preferably, the oxidized sodium alginate is prepared by mixing sodium periodate and sodium alginate and then oxidizing them; wherein, in the mixed solution of sodium periodate and sodium alginate, the concentration of the sodium alginate is 5.4*10 -3 ~1.2*10 -2 g / mL, the concentration of sodium periodate is 1.0*10 -2 ~1.2*10 -2 g / mL.

[0016] Preferably, the viscosity of the sodium alginate is 350-400 mPa.s.

[0017] Preferably, the oxidation degree of the oxidized sodium alginate is 48% to 55%.

[0018] Preferably, in step S1, after the 2-morphineethanesulfonic acid solution of N-carboxyethyl chitosan is added to the mixed solution, the mass fraction of the N-carboxyethyl chitosan is 1.5wt% to 2.5wt%; in step S2, in the PBS solution of oxidized sodium alginate, the mass fraction of oxidized sodium alginate is 0.5wt% to 1.5wt%.

[0019] A fluorescent self-healing injectable hydrogel is prepared by the method.

[0020] Compared with the prior art, the present invention has the following beneficial technical effects:

[0021] The present invention uses co-doped nitrogen and sulfur (N, S-CDs) carbon dots, which have significant fluorescence properties, and its main component 5-oxo-3,5-dihydrothiazole-3,2-pyridine-7-carboxylate sodium (TPCNa) has good biocompatibility. The present invention modifies the bioluminescent small molecules onto the N-carboxyethyl chitosan macromolecular chain through a coupling reaction, and crosslinks the bioluminescent molecules / N-carboxyethyl chitosan polymer with oxidized sodium alginate in situ through a reversible dynamic imine group, thereby obtaining the fluorescent self-healing injectable hydrogel in the present invention. At the same time, in the present invention, the bioluminescent molecules are combined with the hydrogel through chemical bonding coupling, so that the dispersion of the fluorescent substance in the hydrogel is more uniform, and fluorescence quenching is effectively avoided. This fluorescent self-healing injectable hydrogel not only has the self-healing, injectable, biocompatibility and biodegradability of the polysaccharide-based dynamic hydrogel, but also has the non-invasive real-time monitoring function brought by the photoluminescent performance. The fluorescent self-healing injectable hydrogel provided by the present invention is easy to prepare, has mild reaction conditions, and has excellent biocompatibility, and has great application prospects in the field of biological imaging of minimally invasive interventional treatment technology.

[0022] Furthermore, the preparation of the bioluminescent molecule is specifically as follows: citric acid powder and cysteine ​​are uniformly mixed, heated for reaction, the product is washed, and then recrystallized to obtain the bioluminescent molecule, and the obtained bioluminescent molecule has good cell compatibility and tissue compatibility.

[0023] Furthermore, the N-carboxyethyl chitosan is prepared by mixing chitosan and acrylic acid and reacting them, which can improve the water solubility of chitosan; wherein, in the mixed solution of chitosan and acrylic acid, the concentration of chitosan is 5-10mM, and the concentration of acrylic acid is 20-25mM, which can make the grafting degree of chitosan meet the use requirements.

[0024] Furthermore, the deacetylation degree of the chitosan is 86% to 88%, and the molecular weight of the chitosan is 2*10 5 ~3*10 5 g / mol, which can make chitosan have moderate viscosity and can form hydrogel well.

[0025] Furthermore, the amino substitution degree of the N-carboxyethyl chitosan is 48% to 50%, which can improve the water solubility of chitosan while retaining a certain amount of amino groups.

[0026] Furthermore, the oxidized sodium alginate is prepared by mixing sodium periodate and sodium alginate and then oxidizing them, so that the sodium alginate molecule contains a certain aldehyde group; wherein, in the mixed solution of sodium periodate and sodium alginate, the concentration of the sodium alginate is 5.4*10 -3 ~1.2*10 -2 g / mL, the concentration of sodium periodate is 1.0*10 -2 ~1.2*10-2 g / mL, sodium periodate can only oxidize part of the hydroxyl groups of sodium alginate.

[0027] Furthermore, the viscosity of the sodium alginate is 350-400 mPa.s, which enables the sodium alginate to form a hydrogel well.

[0028] Furthermore, the oxidation degree of the oxidized sodium alginate is 48% to 55%, which allows the aldehyde groups on the sodium alginate to form appropriate imine bonds with the amino groups on the chitosan.

[0029] Furthermore, in step S1, after the 2-morphineethanesulfonic acid solution of N-carboxyethyl chitosan is added to the mixed solution, the mass fraction of the N-carboxyethyl chitosan is 1.5wt% to 2.5wt%, which allows the chitosan to be well dispersed and dissolved; in step S2, in the PBS solution of oxidized sodium alginate, the mass fraction of oxidized sodium alginate is 0.5wt% to 1.5wt%, which allows the viscosity of the oxidized sodium alginate to be moderate. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0031] Figure 1 It is a schematic diagram of a process for preparing a fluorescent self-healing injectable hydrogel in the present invention;

[0032] Figure 2 is a reaction formula for synthesizing the bioluminescent molecule (i), oxidized sodium alginate (ii), N-carboxyethyl chitosan, and the bioluminescent molecule / N-carboxyethyl chitosan polymer (iii) in the present invention;

[0033] Figure 3A The oscillation frequency scan of the TPCNa / CEC-I-OSA hydrogel prepared in Example 1 of the present invention;

[0034] Figure 3B The oscillatory strain scan of the TPCNa / CEC-I-OSA hydrogel prepared in Example 1 of the present invention;

[0035] Figure 3C The rheological recovery test results of the TPCNa / CEC-I-OSA hydrogel prepared in Example 1 of the present invention;

[0036] Figure 4AThe TPCNa / CEC-I-OSA hydrogel prepared in Example 1 of the present invention was injected through needles of different sizes (26g, 25g, 22g, 20g);

[0037] Figure 4B This is a photo showing the self-healing performance of a cartoon bear's head constructed by TPCNa / CEC-I-OSA hydrogel prepared by an embodiment of the present invention;

[0038] Figure 5A The photoluminescence photos and spectrum analysis results of TPCNa / CEC-I-OSA hydrogel and TPCNa / CEC solution;

[0039] Figure 5B To analyze the RGB values ​​of the solution and photoluminescent hydrogel photos using image processing software;

[0040] Figure 5C Fluorescence spectrum analysis of TPCNa / CEC-I-OSA hydrogel;

[0041] Fig. 6A This is a picture showing the effect of injecting TPCNa / CEC-I-OSA hydrogel on the back of mice;

[0042] Figure 6B The biodegradation of fluorescent self-healing injectable hydrogel in mice;

[0043] Figure 7 H&E staining of subcutaneous skin tissue and muscle tissue after injection of TPCA / CEC-OSA hydrogel. DETAILED DESCRIPTION

[0044] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0045] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0046] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0047] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0048] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0049] like Figure 1 As shown, the present invention provides a method for preparing a fluorescent self-healing injectable hydrogel, comprising the following steps:

[0050] S1: dissolving the bioluminescent molecule in a 2-morphineethanesulfonic acid solution, then adding 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, stirring and dissolving to obtain a mixed solution; adding a 2-morphineethanesulfonic acid solution of N-carboxyethyl chitosan to the mixed solution, stirring and reacting to obtain a bioluminescent molecule / N-carboxyethyl chitosan polymer;

[0051] Among them, Figure 2 As shown in (i), the preparation process of the bioluminescent molecule (5-oxo-3,5-dihydro-2H-thiazolo[3,2-a]pyridine-7-carboxylic sodium, 5-oxo-3,5-dihydrothiazolidine-3,2-pyridine-7-carboxylic acid sodium, TPCNa) is synthesized by heating a mixture powder of citric acid and cysteine. The specific synthesis process is as follows: citric acid (0.1 mol, 21.01 g) powder and cysteine ​​(0.1 mol, 12.11 g) are uniformly mixed in a beaker, heated to 120-180°C in an oven, and the heating reaction time is at least 3-5 h. During the reaction, as the reaction time changes, the white powder is melted into a transparent concentrated syrup solution, and the color gradually changes from yellow to dark brown. 100 mL of deionized water is added to the beaker, and the precipitate is collected by suction filtration and repeated washing. Finally, the product is dissolved in 200 mL of deionized water, heated at 90°C for recrystallization, and TPCNa crystals are obtained. The typical yield of TPCNa is about 51%.

[0052] The preparation process of N-carboxyethyl chitosan and bioluminescent molecules / N-carboxyethyl chitosan polymers is as follows Figure 2 (iii) as shown.

[0053] The preparation process of N-carboxyethyl chitosan (CEC) is prepared by Michael addition reaction. First, a mixture of chitosan and acrylic acid is prepared, magnetic stirring is performed, the pH value is adjusted, dialyzed in deionized water, and the mixed solution is freeze-dried to obtain N-carboxyethyl chitosan. The specific steps are as follows: First, chitosan is dissolved in distilled water containing acrylic acid to obtain a chitosan acrylic acid mixture, wherein the chitosan is acid-soluble chitosan, the degree of deacetylation is 86% to 88%, and the molecular weight is 2*10 5 ~3*10 5 g / mol; the chitosan concentration in the mixed solution of chitosan and acrylic acid is 5-10mM, the concentration of acrylic acid is 20-25mM, and the mass ratio of chitosan to acrylic acid is controlled to be (0.2-0.25):1. The mixed solution is magnetically stirred at 50-70°C for 3-4 days, and the speed of the magnetic stirring is 90rpm. Then the pH value of the solution is adjusted to 10-12 by dropping 1M NaOH. Subsequently, the solution is dialyzed in deionized water for 3 days, the molecular weight cutoff of the dialysis bag is 8000Da, and the deionized water is replaced twice a day. Finally, CEC is obtained by freeze-drying the solution, and the amino substitution degree of the CEC is 48%-50%.

[0054] Preparation of bioluminescent molecule / N-carboxyethyl chitosan polymer (TPCNa / CEC). TPCNa / CEC luminescent polymer was prepared by a typical carbodiimide coupling reaction, specifically: 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC·HCl) was used as an activator and N-hydroxysuccinimide (NHS) was used as a stabilizer. The specific process is as follows: TPCNa (21.9 mg, 0.1 mmol) was dissolved in 10 mL of 2-morphineethanesulfonic acid solution (MES, pH = 5.5), and EDC·HCl (19.17 mg, 0.1 mmol) and NHS (11.5 mg, 0.1 mmol) were also dissolved in the MES solution to obtain a mixed solution. On the other hand, CEC (200 mg, 0.324 mmol) was completely dissolved in 50 mL of 2-morphineethanesulfonic acid (MES, pH = 5.5) buffer solution. Then the above 10mL TPCNa mixed solution and 50mL CEC solution were mixed, and then a sufficient graft coupling reaction occurred under magnetic stirring at room temperature for 24h. Then, the above mixed solution was transferred to a dialysis bag (MWCO 3500Da) for 7 days, and the water was changed 3 times a day during the dialysis period, and then freeze-dried to obtain a luminescent TPCNa / CEC polymer powder. The grafting rate of TPCNa can be calculated to be 82% by comparing the characteristic proton peak of TPCNa and the characteristic peak area of ​​CEC by nuclear magnetic peak area, and the typical yield of the synthetic reaction calculated by weighing is 69%.

[0055] S2: Mixing the PBS solution of the bioluminescent molecule / N-carboxyethyl chitosan polymer with the PBS solution of oxidized sodium alginate to prepare the fluorescent self-healing injectable hydrogel.

[0056] The synthesis of oxidized sodium alginate (OSA) is as follows: Figure 2 As shown in (ii), oxidized sodium alginate is synthesized by sodium periodate oxidation, that is, sodium alginate, sodium periodate and deionized water are prepared into a reaction solution, and after the oxidation reaction is carried out under light-proof conditions, ethylene glycol is added and stirred to terminate the oxidation reaction, and the mixed solution obtained by the reaction is added to a dialysis bag for dialysis, and then freeze-dried to obtain oxidized sodium alginate.

[0057] Specifically, sodium alginate is dissolved in deionized water, the viscosity of sodium alginate is 350-400 mPa.s, and then sodium periodate is added to obtain a mixed solution. In the mixed solution, the concentration of sodium alginate is 5.4*10 -3 ~1.2*10 -2 g / mL, the concentration of sodium periodate is 1.0*10 -2 ~1.2*10 -2g / mL, and then magnetically stirred for 5-6 hours at 20-25°C in the dark at a speed of 90 rpm. Then ethylene glycol was added and stirred for 1-2 hours to terminate the oxidation reaction. The final concentration of ethylene glycol in the reaction system was 1.5-2 vol%. The mixture obtained by the reaction was dialyzed in deionized water (MWCO 3000Da) for 3 days, during which the deionized water was replaced twice a day. Finally, OSA was obtained by freeze drying, and the degree of oxidation of the OSA was 48% to 55%.

[0058] OSA and TPCNa / CEC polymer were then dissolved in PBS solution (pH 7.4) to obtain homogeneous solutions. After the two solutions were mixed, TPCNa / CEC-I-OSA hydrogel could be quickly obtained (about 1 min).

[0059] In step S1, after adding the 2-morphineethanesulfonic acid solution of N-carboxyethyl chitosan to the mixed solution, the mass fraction of the N-carboxyethyl chitosan is 1.5wt% to 2.5wt%; in step S2, in the PBS solution of oxidized sodium alginate, the mass fraction of oxidized sodium alginate is 0.5wt% to 1.5wt%.

[0060] The invention provides a method for preparing a fluorescent self-healing injectable hydrogel. The method comprises the following steps: using 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride as an activator and N-hydroxysuccinimide as a stabilizer, bonding a bioluminescent molecule (sodium 5-oxo-3,5-dihydrothiazole-3,2-pyridine-7-carboxylate) to N-carboxyethyl chitosan through a coupling reaction, generating a bioluminescent molecule / N-carboxyethyl chitosan polymer, namely anchoring a biocompatible fluorescent small molecule to a polysaccharide macromolecular chain, and then in situ crosslinking is performed through a dynamic imine bond under physiological conditions, namely in situ crosslinking of the bioluminescent molecule / N-carboxyethyl chitosan polymer and oxidized sodium alginate, thereby obtaining the fluorescent self-healing injectable hydrogel of the invention. In this fluorescent self-healing injectable hydrogel, the bioluminescent molecules have excellent biocompatibility. The bioluminescent molecules are combined with the hydrogel by chemical bonding, which effectively improves the combination effect of the fluorescent substance and the hydrogel. At the same time, the fluorescent substance is bonded to N-carboxyethyl chitosan before the synthesis of the hydrogel, and then combined with oxidized sodium alginate, that is, bonded to the hydrogel by in-situ addition, so that the dispersion of the fluorescent substance in the hydrogel is more uniform. In this scheme, N-carboxyethyl chitosan is used for reaction, which effectively improves the solubility. During the reaction, the amino groups on the macromolecular chain of N-carboxyethyl chitosan react with the aldehyde groups on the macromolecular chain of oxidized sodium alginate to obtain a hydrogel through imine bond crosslinking. In addition, the uniformly dispersed fluorescent substance in this scheme can effectively avoid the fluorescence quenching caused by the aggregation of the fluorescent substance, and effectively enhance the fluorescence performance of the fluorescent substance. Therefore, a self-healing injectable hydrogel with good fluorescence performance is obtained by the above method, which effectively expands the application prospects of self-healing injectable hydrogels in real-time monitoring of non-destructive and in-situ treatment processes. That is, the hydrogel prepared by the present invention has self-healing, injectability, shape adaptability, biodegradability, biocompatibility and fluorescence performance. The preparation method comprises: preparing N-carboxyethyl chitosan (CEC) by Michael addition reaction, and obtaining N-carboxyethyl chitosan (CEC) powder by freeze drying; synthesizing oxidized sodium alginate (OSA), dissolving sodium alginate completely in deionized water, then adding sodium periodate and stirring, and obtaining oxidized sodium alginate powder by freeze drying after dialysis; synthesizing biocompatible luminescent small molecules (TPCNa), and synthesizing TPCNa by heating a mixture powder of citric acid and cysteine. Then, the luminescent small molecule (TPCNa) was used to modify N-carboxyethyl chitosan (CEC) to obtain TPCNa / CEC luminescent polymer. The TPCNa / CEC luminescent polymer was prepared by a typical carbodiimide coupling reaction, and was synthesized under the conditions of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC·HCl) as an activator and N-hydroxysuccinimide (NHS) as a stabilizer. Finally, the oxidized sodium alginate and TPCNa / CEC polymer were dissolved in PBS solution to obtain homogeneous solutions.After the two solutions are mixed, TPCNa / CEC-I-OSA hydrogel can be quickly obtained. That is, the present invention discloses a fluorescent self-healing injectable hydrogel and a preparation method thereof. The biocompatible fluorescent small molecule is anchored to the polysaccharide macromolecular chain through the EDC / NHS coupling reaction, and then in situ cross-linking is performed through dynamic imine bonds under physiological conditions to prepare a fluorescent self-healing injectable hydrogel. The fluorescent self-healing injectable hydrogel has comprehensive characteristics such as self-healing, injectability, shape adaptability, biodegradability, cell compatibility and tissue compatibility, and can be used for non-destructive, in situ, real-time monitoring.

[0061] The bioluminescent small molecule TPCNa in the fluorescent self-healing injectable hydrogel of the present invention has good biocompatibility. The fluorescence characteristics of the bioluminescent small molecule TPCNa come from the carbon dots co-doped with nitrogen and sulfur (N, S-CDs), and the fluorescence characteristics are significant. The bioluminescent small molecule TPCNa is further modified on the polymer chain of the CEC biomacromolecule through a coupling reaction, and the bonding is stable and the fluorescence dispersion effect is good. The amino group (-NH 2 ) and the aldehyde groups (-CHO) hanging on OSA form reversible cross-links through Schiff base reaction, and the obtained hydrogel has excellent mechanical properties, injectability, self-healing properties and biocompatibility.

[0062] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0063] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0064] Example 1

[0065] Step 1: Preparation of N-carboxyethyl chitosan (CEC) via Michael addition reaction.

[0066] The specific steps are as follows: first, dissolve chitosan in distilled water containing acrylic acid to obtain a chitosan-acrylic acid mixed solution after dissolution, wherein the concentration of chitosan in the chitosan-acrylic acid mixed solution is 6.2mM, and the concentration of acrylic acid in the chitosan-acrylic acid mixed solution is 21.3mM; magnetic stirring is performed at 50°C for 3 days, and the speed of the magnetic stirring is 90rpm. Then, the pH value of the solution is adjusted to 11 by dropping 1M NaOH. For the next 3 days, the solution is dialyzed in deionized water (MWCO8000Da), during which the deionized water is replaced twice a day. Finally, CEC is obtained by freeze-drying the solution, and the amino substitution degree of the CEC is 48%.

[0067] Step 2: Synthesize oxidized sodium alginate (OSA) by oxidation with sodium periodate.

[0068] The specific steps are as follows: 1.0g of sodium alginate is dissolved in 100mL of deionized water, wherein the viscosity of the sodium alginate is greater than 350mPa.s, 1.08g of sodium periodate is added, and magnetic stirring is performed at 25°C under light-proof conditions for 5h at a speed of 90rpm. Then 1.5mL of ethylene glycol is added and stirred for another 1h to terminate the oxidation reaction. The resulting mixture is dialyzed in deionized water (MWCO 3000Da) for 3 days, during which the deionized water is replaced twice a day. Finally, OSA is obtained by freeze drying, and the degree of oxidation of the obtained OSA is 50%.

[0069] Step 3: Synthesis of biocompatible luminescent small molecules (TPCNa)

[0070] TPCNa is synthesized by heating a mixture powder of citric acid and cysteine. The synthesis process is as follows: citric acid (0.1 mol, 21.01 g) powder and cysteine ​​(0.1 mol, 12.11 g) are evenly mixed in a beaker and heated in an oven at 150 ° C for 3 h. During the reaction, as the reaction time changes, the white powder is melted into a transparent thick syrup solution, and the color gradually changes from yellow to dark brown. 100 mL of deionized water is added to the beaker, and the precipitate is collected by suction filtration and repeated washing. Finally, the product is dissolved in 200 mL of deionized water and heated at 90 ° C for recrystallization to obtain TPCNa crystals. The typical yield of TPCNa is about 51%.

[0071] Step 4: Modification of luminescent small molecules (TPCNa) with N-carboxyethyl chitosan (CEC) and preparation of TPCNa / CEC-I-OSA hydrogel

[0072] The TPCNa / CEC luminescent polymer was prepared by a typical carbodiimide coupling reaction, and was synthesized under the conditions of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC·HCl) as an activator and N-hydroxysuccinimide (NHS) as a stabilizer. The specific process is as follows: TPCNa (21.9 mg, 0.1 mmol) was dissolved in 10 mL of 2-morphineethanesulfonic acid solution (MES, pH = 5.5), and EDC·HCl (19.17 mg, 0.1 mmol) and NHS (11.5 mg, 0.1 mmol) were also dissolved in the MES solution to obtain a dissolved mixed solution. On the other hand, CEC (200 mg, 0.324 mmol) was completely dissolved in 50 mL of 2-morphineethanesulfonic acid (MES, pH = 5.5) buffer solution. Then, the above 10 mL TPCNa mixed solution and 50 mL CEC solution were mixed, and then a sufficient graft coupling reaction occurred under magnetic stirring at room temperature for 24 h. Then, the above mixed solution was transferred to a dialysis bag (MWCO 3500Da) for 7 days, and the water was changed 3 times a day during the dialysis period, and then freeze-dried to obtain a luminescent TPCNa / CEC polymer powder. By comparing the characteristic proton peak of TPCNa and the characteristic peak area of ​​CEC by NMR peak area, it can be calculated that the grafting rate of TPCNa is 82%, and the typical yield of this synthesis reaction is 69% by weighing.

[0073] OSA and TPCNa / CEC polymer were dissolved in PBS solution (phosphate buffer, pH 7.4) to obtain homogeneous solutions. After the two solutions were mixed, TPCNa / CEC-I-OSA hydrogel could be quickly obtained (about 1 min).

[0074] Example 2

[0075] This embodiment provides a method for preparing a fluorescent self-healing injectable hydrogel. The preparation method described in the present invention refers to Example 1. The oxidation degree of the prepared oxidized sodium alginate is 50%, and the amino substitution degree of the prepared N-carboxyethyl chitosan is 48%; the grafting rate of TPCNa is 80%, and the typical yield of this synthesis reaction calculated by weighing is 67%.

[0076] Example 3

[0077] This embodiment provides a method for preparing a fluorescent self-healing injectable hydrogel. The preparation method described in the present invention refers to Example 1. The oxidation degree of the prepared oxidized sodium alginate is 55%, and the amino substitution degree of the prepared N-carboxyethyl chitosan is 50%. The grafting rate of TPCNa is 81%, and the typical yield of this synthetic reaction calculated by weighing is 68%.

[0078] Example 4

[0079] A method for preparing a fluorescent self-healing injectable hydrogel comprises the following steps:

[0080] (1) Preparation of bioluminescent molecule TPCNa: 21.01 g of citric acid powder and 12.11 g of cysteine ​​were uniformly mixed in a beaker, heated to 120°C in an oven, and the heating reaction time was 3 h. After the reaction was completed, 100 mL of deionized water was added to the beaker, and the product was filtered, washed, and the precipitate was collected. Finally, the product was dissolved in 200 mL of deionized water and heated at 90°C for recrystallization to obtain TPCNa crystals.

[0081] (2) Preparation of N-carboxyethyl chitosan (CEC): Chitosan was dissolved in distilled water containing acrylic acid to obtain a chitosan-acrylic acid mixed solution, wherein the chitosan was acid-soluble chitosan with a deacetylation degree of 86% and a molecular weight of 2*10 5 g / mol; the chitosan concentration in the mixed solution of chitosan and acrylic acid is 5mM, and the acrylic acid concentration is 20mM. The mixed solution is magnetically stirred at 50°C for 4 days, and the speed of the magnetic stirring is 90rpm. Then the pH value of the solution is adjusted to 10 by dropping 1M NaOH. Subsequently, the solution is dialyzed in deionized water for 3 days, and the molecular weight cutoff of this dialysis bag is 8000Da. During this period, the deionized water is replaced twice a day. Finally, CEC is obtained by freeze-drying the solution, and the amino group of the CEC.

[0082] (3) Preparation of bioluminescent molecule / N-carboxyethyl chitosan polymer (TPCNa / CEC): TPCNa (21.9 mg, 0.1 mmol) was dissolved in 10 mL of 2-morphineethanesulfonic acid solution (MES, pH = 5.5), and EDC·HCl (19.17 mg, 0.1 mmol) and NHS (11.5 mg, 0.1 mmol) were also dissolved in the MES solution to obtain a dissolved mixed solution. On the other hand, CEC (200 mg, 0.324 mmol) was completely dissolved in 50 mL of 2-morphineethanesulfonic acid (MES, pH = 5.5) buffer solution. Then, the above 10 mL of TPCNa mixed solution and 50 mL of CEC solution were mixed, and then a sufficient graft coupling reaction occurred under magnetic stirring at room temperature for 24 h. Then, the mixed solution was transferred to a dialysis bag (MWCO 3500Da) and dialyzed for 7 days, during which the water was changed 3 times a day, and then freeze-dried to obtain the luminescent TPCNa / CEC polymer powder.

[0083] (4) Preparation of oxidized sodium alginate (OSA): Sodium alginate was dissolved in deionized water, the viscosity of sodium alginate was 350 mPa.s, and then sodium periodate was added to obtain a mixed solution. The concentration of sodium alginate in the mixed solution was 5.4*10 -3 g / mL, the concentration of sodium periodate is 1.0*10 -2 g / mL, and then magnetically stirred for 6 hours at 20°C in the dark at a speed of 90 rpm. Then ethylene glycol was added and stirred for another 2 hours to terminate the oxidation reaction. The final concentration of ethylene glycol in the reaction system was 1.5 vol%. The mixture obtained by the reaction was dialyzed in deionized water (MWCO 3000Da) for 3 days, during which the deionized water was replaced twice a day. Finally, OSA was obtained by freeze drying, and the degree of oxidation of the obtained OSA was 48%.

[0084] (5) OSA and TPCNa / CEC polymer were then dissolved in PBS solution (pH 7.4) to obtain homogeneous solutions. The two solutions were mixed to obtain TPCNa / CEC-I-OSA hydrogel.

[0085] In step S1, after adding the 2-morphineethanesulfonic acid solution of N-carboxyethyl chitosan to the mixed solution, the mass fraction of the N-carboxyethyl chitosan is 1.5wt%; in step S2, in the PBS solution of oxidized sodium alginate, the mass fraction of oxidized sodium alginate is 0.5wt%.

[0086] Example 5

[0087] A method for preparing a fluorescent self-healing injectable hydrogel comprises the following steps:

[0088] (1) Preparation of bioluminescent molecule TPCNa: 21.01 g of citric acid powder and 12.11 g of cysteine ​​were uniformly mixed in a beaker, heated to 180°C in an oven, and the heating reaction time was 5 h. After the reaction was completed, 100 mL of deionized water was added to the beaker, and the product was filtered, washed, and the precipitate was collected. Finally, the product was dissolved in 200 mL of deionized water and heated at 90°C for recrystallization to obtain TPCNa crystals.

[0089] (2) Preparation of N-carboxyethyl chitosan (CEC): Chitosan was dissolved in distilled water containing acrylic acid to obtain a chitosan-acrylic acid mixed solution, wherein the chitosan was acid-soluble chitosan with a deacetylation degree of 88% and a molecular weight of 3*10 5g / mol; the chitosan concentration in the mixed solution of chitosan and acrylic acid is 10mM, and the concentration of acrylic acid is 25mM. The mixed solution is magnetically stirred at 70°C for 3 days, and the speed of the magnetic stirring is 90rpm. Then the pH value of the solution is adjusted to 12 by dropping 1M NaOH. Subsequently, the solution is dialyzed in deionized water for 3 days, and the molecular weight cutoff of the dialysis bag is 8000Da. During this period, the deionized water is replaced twice a day. Finally, CEC is obtained by freeze-drying the solution, and the amino substitution degree of the CEC is 50%.

[0090] (3) Preparation of bioluminescent molecule / N-carboxyethyl chitosan polymer (TPCNa / CEC): 21.9 mg of TPCNa was dissolved in 10 mL of 2-morphineethanesulfonic acid solution (MES, pH = 5.5), and 19.17 mg of EDC·HCl and 11.5 mg of NHS were also dissolved in the MES solution to obtain a dissolved mixed solution. On the other hand, 200 mg of CEC was completely dissolved in 50 mL of 2-morphineethanesulfonic acid (MES, pH = 5.5) buffer solution. Then, the above 10 mL of TPCNa mixed solution and 50 mL of CEC solution were mixed, and then a sufficient graft coupling reaction occurred under magnetic stirring at room temperature for 24 hours. Then, the above mixed solution was transferred to a dialysis bag (MWCO 3500Da) and dialyzed for 7 days. The water was changed 3 times a day during the dialysis period, and then freeze-dried to obtain the luminescent TPCNa / CEC polymer powder.

[0091] (4) Preparation of oxidized sodium alginate (OSA): Sodium alginate was dissolved in deionized water. The viscosity of sodium alginate was 400 mPa.s. Then sodium periodate was added to obtain a mixed solution. The concentration of sodium alginate in the mixed solution was 1.2*10 -2 g / mL, the concentration of sodium periodate is 1.2*10 -2 g / mL, and then magnetically stirred for 5 hours at 25°C in the dark at a speed of 90 rpm. Then ethylene glycol was added and stirred for another 2 hours to terminate the oxidation reaction. The final concentration of ethylene glycol in the reaction system was 2 vol%. The mixture obtained by the reaction was dialyzed in deionized water (MWCO 3000Da) for 3 days, during which the deionized water was replaced twice a day. Finally, OSA was obtained by freeze drying, and the degree of oxidation of the obtained OSA was 55%.

[0092] (5) OSA and TPCNa / CEC polymer were then dissolved in PBS solution (pH 7.4) to obtain homogeneous solutions. The two solutions were mixed to obtain TPCNa / CEC-I-OSA hydrogel.

[0093] In step S1, after adding the 2-morphineethanesulfonic acid solution of N-carboxyethyl chitosan to the mixed solution, the mass fraction of the N-carboxyethyl chitosan is 2.5wt%; in step S2, in the PBS solution of oxidized sodium alginate, the mass fraction of oxidized sodium alginate is 1.5wt%.

[0094] Example 6

[0095] A method for preparing a fluorescent self-healing injectable hydrogel comprises the following steps:

[0096] (1) Preparation of bioluminescent molecule TPCNa: 21.01 g of citric acid powder and 12.11 g of cysteine ​​were uniformly mixed in a beaker, heated to 150°C in an oven, and the heating reaction time was 4 h. After the reaction was completed, 100 mL of deionized water was added to the beaker, and the product was filtered, washed, and the precipitate was collected. Finally, the product was dissolved in 200 mL of deionized water and heated at 90°C for recrystallization to obtain TPCNa crystals.

[0097] (2) Preparation of N-carboxyethyl chitosan (CEC): Chitosan was dissolved in distilled water containing acrylic acid to obtain a chitosan-acrylic acid mixed solution, wherein the chitosan was acid-soluble chitosan with a deacetylation degree of 87% and a molecular weight of 2.5*10 5 g / mol; the chitosan concentration in the mixed solution of chitosan and acrylic acid is 7mM, and the acrylic acid concentration is 22mM. The mixed solution is magnetically stirred at 60°C for 3 days, and the speed of the magnetic stirring is 90rpm. Then the pH value of the solution is adjusted to 11 by adding 1M NaOH. Subsequently, the solution is dialyzed in deionized water for 3 days, and the molecular weight cutoff of the dialysis bag is 8000Da. During this period, the deionized water is replaced twice a day. Finally, CEC is obtained by freeze-drying the solution, and the amino substitution degree of the CEC is 49%.

[0098] (3) Preparation of bioluminescent molecule / N-carboxyethyl chitosan polymer (TPCNa / CEC): 21.9 mg of TPCNa was dissolved in 10 mL of 2-morphineethanesulfonic acid solution (MES, pH = 5.5), and 19.17 mg of EDC·HCl and 11.5 mg of NHS were also dissolved in the MES solution to obtain a dissolved mixed solution. On the other hand, 200 mg of CEC was completely dissolved in 50 mL of 2-morphineethanesulfonic acid (MES, pH = 5.5) buffer solution. Then, the above 10 mL of TPCNa mixed solution and 50 mL of CEC solution were mixed, and then a sufficient graft coupling reaction occurred under magnetic stirring at room temperature for 24 hours. Then, the above mixed solution was transferred to a dialysis bag (MWCO 3500Da) and dialyzed for 7 days. The water was changed 3 times a day during the dialysis period, and then freeze-dried to obtain the luminescent TPCNa / CEC polymer powder.

[0099] (4) Preparation of oxidized sodium alginate (OSA): Sodium alginate was dissolved in deionized water, the viscosity of sodium alginate was greater than 350 mPa.s, and then sodium periodate was added to obtain a mixed solution. In the mixed solution, the concentration of sodium alginate was 1.0*10 -2 g / mL, the concentration of sodium periodate is 1.1*10 -2 g / mL, and then magnetically stirred for 5.5 hours at 90 rpm under light-proof conditions at 22°C. Ethylene glycol was then added and stirred for another hour to terminate the oxidation reaction. The final concentration of ethylene glycol in the reaction system was 1.7 vol%. The resulting mixture was dialyzed in deionized water (MWCO 3000Da) for 3 days, during which the deionized water was replaced twice a day. OSA was finally freeze-dried to obtain an oxidation degree of 50%.

[0100] (5) OSA and TPCNa / CEC polymer were then dissolved in PBS solution (pH 7.4) to obtain homogeneous solutions. The two solutions were mixed to obtain TPCNa / CEC-I-OSA hydrogel.

[0101] In step S1, after adding the 2-morphineethanesulfonic acid solution of N-carboxyethyl chitosan to the mixed solution, the mass fraction of the N-carboxyethyl chitosan is 2.0wt%; in step S2, in the PBS solution of oxidized sodium alginate, the mass fraction of oxidized sodium alginate is 1.3wt%.

[0102] The performance of the TPCNa / CEC-I-OSA hydrogel obtained in Example 1 of the present invention was tested by the following method:

[0103] Test 1: Rheological test of TPCNa / CEC-I-OSA hydrogel

[0104] The rheology of the TPCNa / CEC-I-OSA hydrogel obtained in Example 1 was tested, that is, the mechanical properties of the TPCNa / CEC-I-OSA hydrogel were quantitatively evaluated by frequency scanning. The test results are as follows: Figure 3A As shown in Figure 2, the fluorescent hydrogel exhibits an almost constant storage modulus (G'). When the strain is kept at γ = 1.0%, the storage modulus changes from 0.1 to 100 rad·s -1 The entire dynamic frequency sweep changes in the range, and the storage modulus is significantly higher than the corresponding loss modulus (Loss modulus, G”). These data show that the hydrogel exhibits a typical gel state, and the TPCNa / CEC-I-OSA hydrogel has almost no frequency dependence in the tested range, indicating that there are enough dynamically reversible imine bonds in the polymer network to form a stable hydrogel.

[0105] The linear viscoelasticity of the hydrogel was further studied by strain oscillation rheology experiments. Figure 3B As shown. Figure 3B It can be seen that under low strain (1% to 80%), the hydrogel exhibits linear viscoelastic behavior, while the storage modulus and loss modulus remain unchanged and are independent of the strain amplitude. γ = 80%, which is the critical strain point for the storage modulus and loss modulus values. Due to the dissociation of some reversible imine bonds under relatively high strains, the TPCNa / CEC-I-OSA hydrogel is in a gel-sol state. This critical point shows that when γ < 80%, the hydrogel exhibits elastic gel behavior of an associated or cross-linked polymer network; when γ > 80%, with the further increase of strain, a sudden decrease in the storage modulus value and a rapid increase in the loss modulus value are observed, indicating that the dynamic hydrogel undergoes a gel-sol transition from a solid state with gel properties to a fluid state. The results show that the rheological behavior and injectability of the hydrogel can be adjusted by adjusting the strain to induce shear thinning of the hydrogel.

[0106] The reversibility of the hydrogel gel-sol transition was further verified by rheological recovery performance testing, revealing the dynamic self-healing behavior of the fluorescent hydrogel. Figure 3C As shown. Figure 3C It can be seen that the hydrogel undergoes gel-sol state transition under low shear strain (1%, 200s) and high shear strain (800%, 200s) cycles. When the shear strain increases from 1% to 800%, the reversible imine bonds of the hydrogel dissociate under shear thinning, and the storage modulus decreases by about two orders of magnitude in value. When the shear strain decreases from 800% to 1%, the imine bonds of the hydrogel reform, and the storage modulus almost completely recovers to the initial level of the gel state.

[0107] The above experimental results show that the gel-sol transition of fluorescent hydrogel is reversible and can heal itself to its original state without affecting the mechanical properties. The cross-linking and dissociation process of the abundant dynamic imine bonds in the polysaccharide chain is the reason why the fluorescent hydrogel exhibits rapid alternating stress relaxation.

[0108] Test 2: Self-healing performance test of TPCNa / CEC-I-OSA hydrogel

[0109] The hydrogel can be injected into the syringe using needles of different sizes (20g, 22g, 25g, 26g), showing the excellent injectability of the fluorescent hydrogel. Figure 4A shown.

[0110] Figure 4B The above figure shows that the almost colorless fluorescent self-healing injectable hydrogel obtained by the present invention is first irradiated with ultraviolet light. The results show that after irradiation, the hydrogel appears bright blue. At the same time, after 10 minutes, the cartoon panda head formed by the hydrogel is lifted up, and it is found that the hydrogel has strong mechanical properties. In addition, Figure 4B The figure below shows the dyeing of the hydrogel. One part is dyed with methylene blue to serve as the face of the cartoon panda, and the other part is dyed pink with eosin dye to serve as the ears of the cartoon panda. After the pink ear hydrogel is brought into contact with the blue face hydrogel, the pink and blue parts can heal themselves without any external intervention, and the completed cartoon panda pattern is obtained ( Figure 4B iii), and can withstand large deformation and stretching after 10 minutes ( Figure 4B iv), by reshaping and integrating the cartoon panda head and the bear head, it was demonstrated from a macroscopic perspective that the hydrogel has the functions of injectability and self-healing. In order to further prove that the cartoon bear can maintain its integrity after self-healing, a simple lifting test was conducted. That is, the two ears that were healed with the face were lifted with tweezers. It can be observed that the boundary of the healed part has obvious deformation, but no splitting was observed, indicating that the two ears are completely fused with the face as a whole, and the cracks tend to be smooth and almost disappear after 30 minutes, and the boundary between the ear and the head becomes blurred ( Figure 4B iv). The results showed that the combined hydrogel had good self-healing properties and remained stable as a whole, and could withstand slight stretching and deformation caused by the weight of the face. This was mainly attributed to the "mobile phase" healing process, including the rapid flow of polymer chains around the damaged area and the automatic dissociation-binding reaction of the dynamic imine bonds between the amino and aldehyde groups on the TPCNa / CEC and OSA biomacromolecules.

[0111] Test 3: Fluorescence performance test of TPCNa / CEC-I-OSA hydrogel

[0112] The photoluminescence properties were evaluated by in situ gelation in a quartz cuvette. Figure 5A The results show that the transparent TPCNa / CEC-I-OSA hydrogel emits very bright purple-blue fluorescence under ultraviolet light (λ = 365nm), which is very similar to the PBS solution of TPCNa / CEC. In order to evaluate the difference in fluorescence intensity in color, the RGB color was analyzed using image processing software and compared with the PBS solutions of TPCNa / CEC and TPCNa / CEC-I-OSA. The results are shown in Figure 2. Figure 5B As shown. Figure 5B It can be seen that the two samples present similar color states, that is, the B value is higher than the R value and the G value, indicating that the photoluminescent hydrogel presents a stronger purple-blue color. In addition, the fluorescent color is evenly distributed in the hydrogel, and the RGB value analysis further confirms this phenomenon. TPCNa is stably connected to the CEC polymer chain, which can effectively block the aggregation of fluorophores in the hydrogel matrix. After gelation, the distribution of TPCNa in the hydrogel matrix is ​​uniform and stable.

[0113] The optimal excitation (Eex) and emission (Eem) wavelengths of the fluorescent hydrogel are 360 ​​nm and 434 nm, respectively. The numerical results are very close to those of the PBS solution of TPCNa / CEC (Eex = 360 nm, Eem = 433 nm), but slightly different from TPCNa (Eex = 339 nm, Eem = 418 nm). This may be due to the chemical reaction between TPCNa and CEC, which has little effect on its photoluminescence properties. The excitation-related emission spectrum of TPCNa / CEC-I-OSA hydrogel is shown in Figure 2. Figure 5C As shown. Figure 5C It can be seen that when the excitation wavelength increases from 300nm to 360nm, the emission wavelength of the photoluminescent hydrogel hardly changes, while the corresponding photoluminescence intensity increases. When the excitation wavelength is further increased to 375nm and 390nm, the corresponding emission wavelength drops sharply. At the same time, when the excitation wavelength is 390nm, the maximum emission wavelength shifts to around 450nm. The above results indicate that the multifunctional hydrogel exhibits fluorescence properties similar to TPCNa because the biocompatible organic fluorophore is stably grafted onto the CEC polymer chain through chemical modification.

[0114] Test 4: Testing of the in vivo injectability and degradability of TPCNa / CEC-I-OSA hydrogel

[0115] Using rats as a model, the hydrogels can be successfully implanted into their bodies by injection, and the shape of the hydrogels can be clearly observed on the dorsal skin of the mice, e.g. Fig. 6A The real-time monitoring of biodegradable hydrogels was analyzed using Balb / c mice as a model. The experimental process is as follows Figure 6BAs shown. The degradation of TPCNa / CEC-I-OSA fluorescent hydrogel in vivo was analyzed by subcutaneous injection on the back of mice. The hydrogel can be smoothly injected into the back of mice, and fluorescence can be observed under ultraviolet light. Subcutaneous bioimaging confirmed that the hydrogel has a sufficiently strong fluorescence intensity. After 42 days, as the size of the hydrogel decreased, the fluorescence intensity also decayed. This shows that the subcutaneously injected hydrogel gradually degrades over time ( Figure 6B ), and it takes a long time to be completely degraded. The results show that fluorescence intensity and in vivo bioimaging can be used as indicators of biodegradation of hydrogels.

[0116] Test 5: Test of biocompatibility of TPCNa / CEC-I-OSA hydrogel

[0117] like Figure 7 As shown in the figure, live-dead staining showed that the released cells still showed high cell viability after growing on the culture dish surface for 72 hours, indicating that the fluorescent hydrogel has excellent cell compatibility. The hydrogel was injected into the back of mice to study the effects on skin and muscle tissues and further evaluate the tissue compatibility of the hydrogel. Figure 7 a. Glutaraldehyde cross-linked chitosan hydrogel (Chitosanhydrogel) was used as the negative control group, and CaCl 2 Cross-linked sodium alginate (Alginatehydrogel) was used as the positive control group. Figure 7 As shown in b, Figure 7 b It can be seen that TPCNA / CEC-l-OSA fluorescent hydrogel did not cause any inflammatory response after being injected into mice for 1 day; on the second day, inflammatory cells infiltrated into the tissue containing chitosan hydrogel; on the third day, a large number of inflammatory cells appeared around the tissue. However, the tissue injected with TPCNa / CEC-l-OSA fluorescent hydrogel contained only a small number of inflammatory cells, which was similar to the test results of sodium alginate hydrogel. This shows that TPCNa / CEC-l-OSA fluorescent hydrogel has good tissue compatibility and will not cause obvious inflammatory response.

[0118] H&E staining results of muscle tissue Figure 7 c. Figure 7 c It can be seen that on the first day after injection, no inflammatory reaction occurred in all muscle tissues injected with hydrogels; on the second day, obvious inflammatory reaction occurred around the tissues injected with chitosan hydrogels; after 3 days, the number of inflammatory cells around the tissues injected with chitosan hydrogels increased significantly. However, no obvious inflammatory cell infiltration occurred around the tissues of the other two groups of hydrogels. This shows that TPCNa / CEC-l-OSA fluorescent hydrogel has good biocompatibility in muscle tissues.

[0119] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

[0120] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a fluorescent self-healing injectable hydrogel, It is characterized in that The following steps are involved: S1: dissolving the bioluminescent molecule in a 2-morphineethanesulfonic acid solution, then adding 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride and N-hydroxysuccinimide, stirring and dissolving to obtain a mixed solution; adding a 2-morphineethanesulfonic acid solution of N-carboxyethyl chitosan to the mixed solution, stirring and reacting to obtain a bioluminescent molecule / N-carboxyethyl chitosan polymer; S2: Mixing the PBS solution containing the bioluminescent molecule / N-carboxyethyl chitosan polymer with the PBS solution containing oxidized sodium alginate to prepare the fluorescent self-healing injectable hydrogel.

2. A method for preparing a fluorescent self-healing injectable hydrogel according to claim 1, It is characterized in that The preparation of the bioluminescent molecule is specifically as follows: citric acid powder and cysteine ​​are mixed evenly, heated for reaction, and the product is washed and recrystallized to obtain the bioluminescent molecule.

3. The method for preparing a fluorescent self-healing injectable hydrogel according to claim 1, It is characterized in that The N-carboxyethyl chitosan is prepared by mixing chitosan and acrylic acid and reacting them; wherein, in the mixed solution of chitosan and acrylic acid, the concentration of chitosan is 5-10mM, and the concentration of acrylic acid is 20-25mM.

4. The method for preparing a fluorescent self-healing injectable hydrogel according to claim 3, It is characterized in that The deacetylation degree of the chitosan is 86% to 88%, and the molecular weight of the chitosan is 2*10 5 ~3*10 5 g / mol.

5. The method for preparing a fluorescent self-healing injectable hydrogel according to claim 1, It is characterized in that The amino substitution degree of the N-carboxyethyl chitosan is 48% to 50%.

6. The method for preparing a fluorescent self-healing injectable hydrogel according to claim 1, It is characterized in that The oxidized sodium alginate is prepared by mixing sodium periodate and sodium alginate and then oxidizing them; wherein, in the mixed solution of sodium periodate and sodium alginate, the concentration of the sodium alginate is 5.4*10 -3 ~1.2*10 -2 g / mL, the concentration of sodium periodate is 1.0*10 -2 ~1.2*10 -2 g / mL.

7. The method for preparing a fluorescent self-healing injectable hydrogel according to claim 6, It is characterized in that The viscosity of the sodium alginate is 350-400 mPa.s.

8. The method for preparing a fluorescent self-healing injectable hydrogel according to claim 1, It is characterized in that The oxidation degree of the oxidized sodium alginate is 48% to 55%.

9. The method for preparing a fluorescent self-healing injectable hydrogel according to claim 1, It is characterized in that In step S1, after adding the 2-morphineethanesulfonic acid solution of N-carboxyethyl chitosan to the mixed solution, the mass fraction of the N-carboxyethyl chitosan is 1.5wt% to 2.5wt%; in step S2, in the PBS solution of oxidized sodium alginate, the mass fraction of oxidized sodium alginate is 0.5wt% to 1.5wt%.

10. A fluorescent self-healing injectable hydrogel, It is characterized in that It is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of polysaccharide-based hydrogel crosslinked by dynamic imine linkages

    CN107964105A

  • Dynamic natural polysaccharide-based red fluorescent nano-composite hydrogel doped with carbon dot inclusion compound and preparation method of dynamic natural polysaccharide-based red fluorescent nano-composite hydrogel

    CN118374029A

  • Photoluminescent hydrogel

    US20180071409A1