Nanometer composite insulating material as well as preparation method and application thereof
By mixing isotropic polypropylene with carbon nanoangle and using physical processes such as supercritical CO2 and ultraviolet irradiation, the problems of by-products and metal impurities in existing high-voltage cable insulation materials are solved, and efficient insulation of the materials is achieved. The mechanical and thermal performance is taken into account, which improves breakdown strength and space charge suppression ability.
Patent Information
- Application Number
- CN202411119928.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
Existing high-voltage cable insulating materials such as XLPE produce by-product methane during processing, and metal impurities exist in carbon nanotube materials, which affects the insulation performance and is difficult to take into account both insulation, mechanical and thermal properties.
Isogastric polypropylene is used to mix with carbon nanoangles, and nanocomposite materials are prepared through physical processes such as grinding, supercritical CO2 dispersion and ultraviolet irradiation to avoid the existence of metal impurities and improve the dispersion and performance of the material.
It achieves the good insulation performance, mechanical performance and thermal performance of high-voltage insulating materials, improves the breakdown strength and space charge suppression ability of the material, and reduces production costs.
Smart Images

Figure CN118994657A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of insulating materials, and in particular to a nano composite insulating material and a preparation method and application thereof. Background Art
[0002] Faced with the rapid growth of modern electricity demand, cable voltage levels are constantly increasing, which has put forward new requirements for the insulation, heat resistance, mechanical strength and other performance indicators of high-voltage cable insulation materials.
[0003] Since the 1970s, flexible cross-linked polyethylene (XLPE), which is mainly composed of chemically cross-linked polyethylene molecules, has been used as insulation material for high voltage (HV) power cables. However, the processing of XLPE is relatively complicated and produces greenhouse gas methane (CH 4 ) and other by-products, some of which will still exist inside the cable even after degassing, affecting the mechanical and electrical properties of the cable.
[0004] In addition, XLPE will form space charge accumulation due to impurity ionization. Carbon nanomaterials such as graphene and graphene oxide have a positive effect on the suppression of space charge. However, nanosheet fillers such as graphene and graphene oxide often curl into particles during processing and cannot fully represent the original state, further affecting the unique properties of the material. In order to achieve the effect of suppressing space charge, the amount of added filler must be increased accordingly. Since carbon-based materials themselves have a certain conductivity, the increase in the amount of filler will affect the insulation properties of the material.
[0005] There are three main methods for synthesizing carbon nanotubes: arc discharge method, laser evaporation method and chemical vapor deposition method. Among them, the arc discharge method has a high reaction temperature, a fast growth rate of carbon nanotubes and difficult to control the preparation parameters, so it is difficult to achieve control of its fine structure. Laser evaporation method is now less used due to expensive and complex equipment. Chemical vapor deposition (CVD) is to decompose carbon-containing compounds to provide a carbon source, and then achieve the growth of carbon nanotubes under the action of a metal catalyst. This method has a low growth temperature, easy to control parameters, high product yield and high carbon purity, and is currently the most widely used technology in the industry. However, this preparation method using a metal catalyst will inevitably cause a large amount of metal impurities in the carbon nanotube material. Therefore, the insulation performance of the composite material doped with carbon nanotubes will decrease due to the presence of metal impurities. Obviously, this defect makes carbon nanotubes unsuitable for cable insulation materials. If the carbon nanotubes are pre-treated with a strong acid, some metal impurities can be removed, but the use of a strong acid will destroy the structure of the carbon nanomaterial and cause a large amount of carbon nanomaterial loss.
[0006] Therefore, in order to take into account both environmental protection performance and reliability at higher voltage levels, it is necessary to develop a new type of insulating material. Summary of the invention
[0007] In order to solve the above problems in the prior art, the present invention aims to provide a nanocomposite insulating material and a preparation method and application thereof. The insulating material can have good insulating properties, mechanical properties and thermal properties.
[0008] In order to achieve the above-mentioned object, according to the first aspect of the present invention, a method for preparing a nanocomposite insulating material is provided. The method comprises: mixing isotactic polypropylene and carbon nanohorns, grinding and treating to obtain a mixed material; making the critical CO 2 The first dispersion material is infiltrated into the mixed material to perform auxiliary dispersion treatment to obtain a first dispersion material; the first dispersion material is melted to obtain a molten material; the molten material is irradiated with ultraviolet rays to obtain a second dispersion material; and the second dispersion material is processed and formed to obtain the nanocomposite insulating material.
[0009] Compared with XLPE, isotactic polypropylene (iPP) has better heat resistance, long-term working temperature can reach above 100°C, melting point reaches 170°C, and density is only 0.91g / cm 3 , the lightest among general-purpose plastics; iPP is a non-polar material with excellent corrosion resistance and extremely low water absorption, with a water absorption rate of <0.01%. iPP has excellent insulation performance and high breakdown field strength. Its electrical properties are basically unaffected by environmental humidity, making it an ideal choice for cable insulation materials. In addition, the manufacturing process of iPP material is simple, and the production cost is significantly lower than XLPE. iPP has higher mechanical strength, and its tensile and bending resistance both exceed XLPE. Its elastic modulus is more than 5 times that of XLPE, which also leads to its high hardness and low toughness. The present invention adds carbon nanohorns (CNHs) therein to effectively improve its flexibility.
[0010] CNHs particles are spherical superstructures formed by the aggregation of carbon nanostructures. 2 It consists of a conical closed tip of bonded carbon atoms and a tubular body similar to single-walled carbon nanotubes (SWCNTs). CNHs have a large internal space and a high specific surface area. In addition to improving the flexibility of iPP materials, CNHs can also improve the high-voltage insulation performance of iPP materials, increase the material's alternating current (AC) and direct current (DC) breakdown strength (BDS), and inhibit space charge accumulation.
[0011] Carbon nanohorns can be prepared at room temperature without the use of metal catalysts, so the prepared carbon nanohorns do not contain metal impurities. Therefore, compared with other carbon nanomaterials such as carbon nanotubes, carbon nanohorns are more practical and avoid defects caused by metal impurities. Therefore, preparing composite materials with CNHs and iPP can take into account both the inhibition of space charge accumulation effect and good insulation properties.
[0012] Furthermore, the preparation process of the present invention only involves physical processes and does not involve chemical modification of CNHs, so the inherent properties of CNHs can be retained. 2 It can reduce the viscosity of polymers and make CNHs disperse better. UV irradiation can change the hydrophobicity of the surface of carbon nanohorns, achieving a short-term reversible conversion between hydrophobicity and hydrophilicity. The hydrophilicity is not limited to the relationship between CNHs and water molecules. Its essence is that UV irradiation reduces the surface energy of CNHs, which enhances the ability and tendency of iPP molecules to spread on its surface, that is, increases the "solubility" of CNHs in iPP.
[0013] In some preferred embodiments of the present invention, the weight average molecular weight of the isotactic polypropylene is 100000±10000. Within the above preferred molecular weight range, it is more conducive to taking into account electrical properties, mechanical properties and thermal properties, so that the prepared composite material is suitable for use as an insulating material.
[0014] In some preferred embodiments of the present invention, the amount of carbon nanohorns added to the nanocomposite insulating material is 1 to 20 phr. Preferably, the amount of carbon nanohorns added to the nanocomposite insulating material is 5±0.1 phr. At this preferred amount, the composite material has the best comprehensive performance.
[0015] In some preferred embodiments of the present invention, the auxiliary dispersion treatment comprises: injecting CO into the mixed material. 2 , the temperature is controlled at 32±0.5℃, the pressure is controlled at 73.8~75bar, and maintained for 10min; secondly, the pressure is reduced to 1.01bar at a rate of 10bar / min. Controlling the temperature and pressure within the above range is more conducive to CO 2 Penetrate into the polymer matrix, reduce the viscosity of iPP, and help disperse CNHs. In the process of reducing pressure, it is better to reduce it slowly to avoid CO 2 Quick release to avoid voids or uneven dispersion.
[0016] In some preferred embodiments of the present invention, the intensity of the ultraviolet light is 40±2 μW / cm 2 The above-preferred ultraviolet rays are more conducive to promoting the dispersion of CNHs in iPP.
[0017] In some preferred embodiments of the present invention, ultraviolet irradiation is performed under the condition of stirring and melting the material.
[0018] In some preferred embodiments of the present invention, before melting the first dispersed material, the preparation method further comprises: granulating the first dispersed material to obtain composite granules; and secondly, melting the composite granules to obtain the molten material.
[0019] In some preferred embodiments of the present invention, the granulation comprises: placing the first dispersed material in an extruder, with an extrusion temperature of 195±2°C, an extrusion rate of 350±10kg / h, and a shear force of 100±5kPa. High temperature, high shear force and supercritical CO 2 The combined plasticizing effect of MgO and MgO ensures better dispersion of CNHs throughout the iPP.
[0020] In some preferred embodiments of the present invention, the carbon nanohorn has a diameter of 2 to 5 nm and a length of 40 to 50 nm.
[0021] In some preferred embodiments of the present invention, the grinding process has a rotation speed of 300±5 rpm and a time of 2±0.2 h.
[0022] In some preferred embodiments of the present invention, the processing and molding includes: melting the second dispersed material at 200±5°C for 5 to 6 minutes, then treating it at 200±5°C for 5 to 6 minutes and pressing it into a film; secondly, quenching it at 10±0.5°C and 10±0.5MPa to obtain the nanocomposite insulating material.
[0023] According to another aspect of the present invention, a nanocomposite insulating material obtained by the above-mentioned preparation method is provided.
[0024] In some preferred embodiments of the present invention, the nanocomposite insulating material meets one or a combination of two or more of the following conditions:
[0025] DC breakdown field strength: 435~445kV / mm;
[0026] AC breakdown field strength: 175~185kV / mm;
[0027] Electric field distortion rate: ≤6%;
[0028] Melting temperature: ≥170℃;
[0029] Tensile strength: ≥35.5MPa.
[0030] According to another aspect of the present invention, there is provided a use of the above-mentioned nanocomposite insulating material in a cable insulating layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The SEM morphology of the cross section of the pure iPP sample is shown.
[0032] Figure 2 The SEM morphology of the cross section of the C-iPP 1 sample is shown.
[0033] Figure 3 The SEM morphology of the cross section of C-iPP 5 sample is shown.
[0034] Figure 4 The SEM morphology of the cross section of the C-iPP 10 sample is shown.
[0035] Figure 5 The SEM morphology of the cross section of the C-iPP 20 sample is shown.
[0036] Figure 6 Thermogravimetric curves of nanocomposite insulating materials are shown.
[0037] Figure 7 The tensile strength of the nanocomposite insulation material is shown.
[0038] Figure 8 The breakdown voltage of the nanocomposite insulating material is shown.
[0039] Fig. 9 SEM images of nanocomposite insulating materials obtained under different intensities of ultraviolet irradiation are shown. DETAILED DESCRIPTION
[0040] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0041] Example 1
[0042] This embodiment provides a nanocomposite insulating material, and the preparation method thereof includes:
[0043] S1, CNHs (804118, Merck reagent) was added to iPP (HP602N, Aladdin reagent, weight average molecular weight of 100000) in proportions (1, 5, 10, 20 phr, respectively), and then dry-mixed in a high-energy ball mill and ground at 300 rpm for 2 hours to ensure preliminary dispersion, thereby obtaining a mixed material;
[0044] S2, put the mixed material into a high-pressure container and inject pure CO 2The container is heated to 31°C and the pressure is maintained above 73.8 bar (maximum not exceeding 75 bar) to allow CO 2 Penetrating into the polymer matrix, then reducing the pressure of the container to the standard atmospheric pressure of 1.01 bar at a rate of 10 bar / min while maintaining the temperature, to obtain a first dispersion;
[0045] S3, transferring the first dispersed material to an extruder, setting the extrusion temperature to 195° C., the shear rate to 350 kg / h, the shear force to 100 kPa, using a melt filter at the end of the extruder to remove lumps or impurities, and granulating to obtain composite pellets;
[0046] S4, the composite pellets were melted at 180°C and stirred at 300 rpm in a high temperature magnetic stirrer for 5 min. At the same time, low intensity ultraviolet light (40 μW / cm 2 ) irradiating the mixture to obtain a second dispersion;
[0047] S5, the second dispersion was melted at 200 °C for 5 min, then compression molded at 200 °C and 15 MPa for 5 min, and finally quenched at 10 °C and 10 MPa to prepare film samples, which were named C-iPP 1, C-iPP 5, C-iPP 10, and C-iPP 20 according to the doping ratio.
[0048] Example 2
[0049] The only difference from Example 1 is that the weight average molecular weights of iPP are 50,000 and 200,000 respectively.
[0050] Example 3
[0051] The only difference from Example 1 is that the extrusion temperatures of the extruders are 170° C. and 220° C. respectively.
[0052] Example 4
[0053] The difference from Example 1 is that the UV intensity when dispersing CNHs is 0, 20, and 60 μW / cm 2 .
[0054] Comparative Example 1
[0055] The only difference from Example 1 is that the added fillers are 5 phr of carbon nanotubes (CNT, JENO Tube 8A, JEIO reagent), carbon black (CB, 300J, Ketjenblack reagent), and graphite (014734, Alfa Aesar reagent).
[0056] The prepared nanocomposite insulating material samples can be tested as follows:
[0057] 1. Use a field emission scanning electron microscope (SEM, S4800, Hitachi Instruments) to characterize the cross-sectional morphology of the film samples.
[0058] 2. Thermal performance was evaluated using differential scanning calorimetry (DSC, Q20, TA Instruments) with a temperature range of 50-200 °C, a heating and cooling rate of 5 °C / min, and a N 2 The thermal stability of the samples was measured by thermogravimetric analysis (TGA, Q600, TA Instruments) in an air atmosphere with a temperature range of 20 to 600°C and a heating rate of 5°C / min.
[0059] 3. According to the provisions of GB / T-1040, a universal testing machine (UTM, AGS-X, Shimadzu Instruments) was used to evaluate the tensile properties of the samples at a crosshead speed of 25 mm / min.
[0060] 4. According to the provisions of GB / T1408, the AC and DC breakdown voltages (Breakdown Voltages, BDV) of the samples were measured using a dielectric strength tester (19032 / 19032-P, Chroma Electronics). A sample with a thickness of 150 μm (±10 μm) was fixed between two spherical electrodes with a diameter of 20 mm in silicone oil (to prevent surface flashover), and a ramp voltage with a step length of 2.2 kV / s was applied until breakdown occurred. The scale and shape parameters of BDS were analyzed using Weibull distribution.
[0061] 5. Use a pulsed electroacoustic (PEA) system (Space Charge Measurement System, NISQUARE instrument) to obtain the spatial charge distribution of the sample. At room temperature, the DC field strength is set to -30 kV / mm and the test time is set to 90 min.
[0062] Test Results
[0063] The dispersion of CNHs in iPP was analyzed by SEM. Figure 1 , Figure 2 , Figure 3 , Figure 4 , Figure 5 The cross-sectional morphologies of the samples with CNHs addition amounts of 0, 1, 5, 10, and 20 phr are given respectively. Figure 1 to Figure 5It can be seen that the CNHs in the present invention are well dispersed in the matrix, and no large amount of aggregated particles are observed. This shows that the process of the present invention can ensure good dispersibility of CNHs in iPP without chemically modifying the CNHs.
[0064] The effect of different UV intensities on the dispersibility of CNHs during sample preparation was analyzed by SEM. Fig. 9 The UV irradiation intensity is given as 0, 20, 40, and 60 μW / cm 2 Dispersion of 5phr CNHs in iPP. Fig. 9 It can be seen that when there is no ultraviolet irradiation, CNHs show serious agglomeration phenomenon. When the ultraviolet intensity rises to 20μW / cm 2 When the UV intensity is 40μW / cm 2 When the UV intensity continued to rise to 60 μW / cm 2 When the intensity of ultraviolet light is 40μW / cm 2 It can be seen that UV irradiation can improve the dispersibility of CNHs in iPP, and the improvement effect is stronger when the concentration of CNHs is 5 phr and the UV intensity is 40 μW / cm 2 reaches its maximum.
[0065] The thermal properties of the samples were analyzed by DSC, and the results are shown in Table 1. As shown in Table 1, the melting temperature (T m ) increases significantly with the increase of CNHs content.
[0066] In addition, the thermal stability of the samples under air conditions was tested by thermogravimetric analysis (e.g. Figure 6 The results show that the thermal stability of the sample is significantly improved after doping with CNHs, and the thermal stability is positively correlated with the CNHs content, which makes the iPP material doped with CNHs more advantageous in high-voltage cable insulation applications.
[0067] The tensile strength of the samples was tested by a universal testing machine (such as Figure 7As shown), the test results show that the addition of CNHs helps to improve the tensile strength of the material and is suitable for power cable applications. The material obtained in Example 2 was subjected to SEM and mechanical property tests, and the results are shown in Table 5. The material obtained in Example 3 was subjected to SEM and mechanical property tests, and the results are shown in Table 6. As can be seen from Table 5, CNHs has good dispersibility in iPP materials with a weight average molecular weight of 100,000, and the composite material can maintain good tensile strength. A lower molecular weight helps to improve the impact strength and thermal stability of the material, but will cause the dispersibility of CNHs to deteriorate. Excessive molecular weight will lead to a decrease in the mechanical properties of the material. As can be seen from Table 6, when the extrusion temperature is 195°C, CNHs has good dispersibility and the tensile strength of the composite material is good. Lower extrusion temperatures reduce the fluidity of the polymer and greatly reduce the dispersibility of CNHs; higher extrusion temperatures can increase the fluidity of the polymer, but at the same time will also increase the cracking reaction of the iPP material, thereby reducing the mechanical properties and thermal stability of the material.
[0068] The DC BDS values of iPP nanocomposite samples doped with 5 phr of carbon nanotubes, carbon black, graphite and carbon nanohorns were compared by Weibull distribution diagram. The test results are shown in Table 2. The results show that the BDS value of the sample doped with carbon nanohorns is significantly greater than that of other samples, which indicates that only CNHs can effectively enhance the DC BDS without any chemical treatment, while other types of nanocarbon fillers are not suitable as additives to enhance the DC BDS of iPP.
[0069] The insulation properties of iPP samples doped with CNHs were evaluated by AC and DC voltage breakdown tests at room temperature. Figure 8 As shown. Under AC voltage, the BDS value of the C-iPP 1 sample is 169.3 kV / mm, which is close to the BDS value of the original iPP sample without CNHs doping (163.1 kV / mm). When the CNHs doping amount is 5 phr, the maximum BDS value of the sample is 178.4 kV / mm, and as the CNHs content continues to increase, the BDS value drops rapidly and is lower than the BDS value of the original sample. This is because the average free path of high-energy charge carriers increases, resulting in accelerated polymer chain breakage or the formation of microvoids, which leads to rapid breakdown of the sample. The results obtained under DC voltage are similar to those of AC. The BDS of the C-iPP 5 sample reaches a peak of 443.7 kV / mm, which is 28.7% higher than that of the original iPP sample. It can be seen from the AC and DC breakdown tests that 5 phr CNHs doping can effectively reduce the insulation breakdown of the iPP material, which is speculated to be due to the role of CNHs as a charge carrier trap.
[0070] One of the key issues of high-voltage power cable insulation is the space charge accumulated in the insulating medium, which can cause electric field distortion and insulation aging, thereby shortening the insulation life. The space charge accumulation behavior of CNHs-doped samples was tested using the PEA system, and the results are shown in Tables 3 and 4. During the polarization process, the charge density near the anode and cathode of the CNHs-doped iPP samples increased compared with the original iPP. At the same time, the negative charge (same type) injected from the cathode partially accumulated in the main body of the original iPP sample, and the internal electric field of the original iPP was significantly distorted, exceeding the external electric field of 30 kV / mm. With the increase of CNHs content, the accumulation of space charge inside the sample was significantly suppressed, and the distorted magnetic field inside the sample gradually recovered and became uniform, close to the external magnetic field, and the residual accumulated charge inside the sample was significantly reduced after depolarization.
[0071] Table 1
[0072] sample CNHs content (phr) <![CDATA[Melting temperature T m (°C)]]> Dispersibility of CNHs iPP 0 167.6 - C-iPP 1 1 168.2 good C-iPP 5 5 170.5 good C-iPP 10 10 171.7 good C-iPP 20 20 172.1 good
[0073] Table 2
[0074] Sample (5phr) DC breakdown field strength Carbon Black 423.5kV / mm graphite 435.1kV / mm Carbon Nanotubes 218.7kV / mm Carbon Nanohorns 439.5kV / mm
[0075] Table 3
[0076]
[0077] Table 4
[0078]
[0079]
[0080] Table 5
[0081]
[0082] Table 6
[0083]
[0084] The above test results show that CNHs can enhance the thermal stability and tensile strength of iPP materials, improve the DC BDS and space charge accumulation of iPP materials, and effectively inhibit the internal electric field distortion of materials. In addition, iPP materials themselves have the characteristics of low cost, high recyclability, and better heat resistance and mechanical strength than XLPE. Therefore, iPP materials doped with CNHs are expected to replace XLPE and play an important role in high-voltage power cable insulation applications.
[0085] With the increase of CNHs content, the thermal stability and tensile strength of the samples increase. For insulation performance, when the CNHs content is 5phr, the breakdown strength of the sample is the highest. Compared with pure iPP, the AC and DC BDS of the iPP nanocomposite are increased by 9% and 29%, respectively. Considering that when the CNHs content gradually increases from 5 to 20phr, the thermal stability and tensile strength increase slightly, when CNHs is 5phr, the comprehensive performance of the composite material is the best.
Claims
1. A method for preparing a nanocomposite insulating material, characterized in that: include: The isotactic polypropylene and the carbon nanohorns are mixed and ground to obtain a mixed material; Allowing critical CO2 to penetrate into the mixed material to perform auxiliary dispersion treatment to obtain a first dispersed material; Melting the first dispersed material to obtain a molten material, and irradiating the molten material with ultraviolet light to obtain a second dispersed material; The second dispersed material is processed and shaped to obtain the nanocomposite insulating material.
2. The preparation method according to claim 1, characterized in that: The weight average molecular weight of the isotactic polypropylene is 100000±10000.
3. The preparation method according to claim 1, characterized in that: The carbon nanohorns are added in an amount of 1 to 20 phr in the nanocomposite insulating material.
4. The preparation method according to claim 1, characterized in that: The auxiliary dispersion treatment includes: injecting CO2 into the mixed material, controlling the temperature to 32±0.5°C and the pressure to 73.8-75 bar, and maintaining for 10 minutes; secondly, reducing the pressure to 1.01 bar at a rate of 10 bar / min.
5. The preparation method according to claim 1, characterized in that: The intensity of the ultraviolet light is 40±2μW / cm 2 .
6. The preparation method according to claim 1, characterized in that: Before melting the first dispersed material, the preparation method further comprises: Granulating the first dispersed material to obtain composite granules; Next, the composite pellets are melted to obtain the molten material.
7. The preparation method according to claim 6, characterized in that: The granulation comprises: placing the first dispersed material in an extruder, with an extrusion temperature of 195±2° C., an extrusion rate of 350±10 kg / h, and a shear force of 100±5 kPa.
8. The preparation method according to claim 1, characterized in that: The carbon nanohorn has a diameter of 2 to 5 nm and a length of 40 to 50 nm.
9. The preparation method according to claim 1, characterized in that: The processing and molding comprises: melting the second dispersed material at 200±5°C for 5-6 minutes, then treating at 200±5°C for 5-6 minutes and pressing into a film; secondly, quenching at 10±0.5°C and 10±0.5MPa to obtain the nanocomposite insulating material.
10. A nanocomposite insulating material obtained by the preparation method according to any one of claims 1 to 9.
11. The nanocomposite insulating material according to claim 10, characterized in that: The nanocomposite insulating material meets one or a combination of two or more of the following conditions: DC breakdown field strength: 435~445kV / mm; AC breakdown field strength: 175~185kV / mm; Electric field distortion rate: ≤6%; Melting temperature: ≥170℃; Tensile strength: ≥35.5MPa.
12. Use of the nanocomposite insulating material according to claim 10 or 11 in a cable insulation layer.