Low-dielectric filler, preparation method thereof and low-dielectric LCP (Liquid Crystal Polymer) composite material
Prepare low-dielectric fillers by acid-high temperature treatment of mineral raw materials, combined with LCP resin, solve the problem of excessive dielectric constant of high frequency and low dielectric constant resin, and achieve the balance of dielectric properties and mechanical properties, suitable for 5G high-frequency high-frequency application.
Patent Information
- Application Number
- CN202411197858.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-22
AI Technical Summary
The dielectric constant of existing high-frequency low-dielectric constant resins is still relatively high, and it has not fully met the demands of 5G communication technology for high-frequency and high-speed transmission and signal stability.
Using low-dielectric fillers, mineral raw materials are treated by acid-high temperature to reduce the content of aluminum and magnesium elements, expand the pore size and pore capacity, and prepare low-dielectric materials with dielectric constants between 2.40 and 2.90, and combine them with LCP resin. Low dielectric LCP composite materials are prepared through twin screw extrusion mechanism.
It effectively reduces the dielectric constant of LCP composite materials, improves its comprehensive mechanical properties, and achieves a balance between dielectric and mechanical properties. It is suitable for 5G high-frequency applications.
Abstract
Description
[0001] The invention relates to the technical field of polymer materials, in particular to a low dielectric filler and a preparation method thereof and a low dielectric LCP composite material. Background Art
[0002] High-frequency low dielectric constant resin is a material with low loss, high-frequency response and good electrical properties. It is widely used in microwave communications, wireless networks, radio frequency modules and other fields. With the development of 5G communication technology, the requirements for high-frequency and high-speed transmission and signal stability are increasing. High-frequency low dielectric constant resin has attracted much attention due to its excellent performance. However, its dielectric constant is still relatively high (Dk>3), which fails to fully meet the needs. LCP liquid crystal polymer is a new type of polymer material with unique performance characteristics including good thermal stability (resistant to flow soldering), high rigidity (suitable for preparing thin materials), intrinsic flame retardancy, low degassing, etc. It is considered to be one of the most promising engineering resins in 5G high-frequency applications.
[0003] In the prior art, adding low-dielectric inorganic fillers can effectively reduce the dielectric constant of engineering composite resins. Currently, low-dielectric inorganic fillers are mainly silicon oxide (Dk=4), and one type is to introduce air through hollow glass microspheres or aerogels (Dk=1). Summary of the invention
[0004] The object of the present invention is to provide a low dielectric filler suitable for preparing a low dielectric LCP composite resin.
[0005] The present invention is achieved through the following technical solutions: A low dielectric filler, wherein the particle size of the low dielectric filler is 200-1200 mesh and the specific surface area is 90-330m 2 / g, pore volume 0.05-1.00cc / g, pore diameter 4-16nm, and the total content of aluminum and magnesium elements is less than 5wt%.
[0006] The low dielectric filler is selected from at least one of low dielectric zeolite, low dielectric palygorskite, low dielectric sepiolite and low dielectric diatomaceous earth.
[0007] Specifically, the low dielectric zeolite has a particle size of 200-1200 mesh and a specific surface area of 140-210 m 2 / g, pore volume 0.4-0.9cc / g, pore diameter 5-11nm, and the total content of aluminum and magnesium elements is less than 4wt%; The low dielectric palygorskite has a particle size of 200-1200 mesh and a specific surface area of 220-330 m 2 / g, pore volume 0.70-1.00cc / g, pore diameter 8-15nm, and the total content of aluminum and magnesium elements is less than 4wt%; The low dielectric sepiolite has a particle size of 200-1200 mesh and a specific surface area of 170-300m 2 / g, pore volume 0.70-1.00cc / g, pore diameter 8-14nm, and the total content of aluminum and magnesium elements is less than 5wt%; The low dielectric diatomite has a particle size of 200-1200 mesh and a specific surface area of 90-190 m 2 / g, pore volume 0.05-0.15cc / g, pore diameter 10-16nm, and the total content of aluminum and magnesium elements is less than 2wt%.
[0008] The constant D of the low dielectric filler k =2.40~2.90, dielectric loss Tanδ is 0.0021~0.0050.
[0009] The method for preparing the low dielectric filler of the present invention comprises the following steps: The method is to treat the mineral raw materials by acid-high temperature treatment, specifically, soaking the mineral raw materials in a mixed acid with a concentration of 0.5-1.2M, stirring at 40-60°C for 4-8 hours; washing with distilled water, and then drying; calcining the dried mineral raw materials at 800-1000°C for 4-8 hours; and grinding to obtain a low dielectric filler; The mixed acid comprises HF, HCl and H2SO4, wherein HF accounts for 5-20%, HCl accounts for 5-90%, and H2SO4 accounts for 5-90%; The mineral raw material is selected from at least one of zeolite, sepiolite, palygorskite and diatomite.
[0010] In the preparation method of the present invention, the corrosiveness of HF reduces the stability of the mineral SiO2 structure, effectively improving the reaction effect of other acids on non-silicon oxides (substances with high dielectric constants such as aluminum oxide and magnesium oxide), the addition of H2SO4 can improve the aluminum removal effect, and the addition of HCl can improve the magnesium removal effect. Under the synergistic effect of the three, the aluminum and magnesium removal effect of the mineral raw material can be significantly achieved, and the pore size and pore volume of the structure can be enlarged, so as to obtain the low dielectric filler with the parameters of the present invention.
[0011] The low dielectric filler of the present invention is used for LCP composite material, and the LCP composite material comprises the following components by weight: 60-80 parts of LCP resin; 1-15 parts of the low dielectric filler of the present invention; Other fillers 0-20 parts.
[0012] The other fillers are selected from at least one of glass fiber, sericite and hollow glass microspheres.
[0013] It is possible to choose whether to add 0-3 parts of auxiliary agent according to actual conditions, and the auxiliary agent is selected from at least one of an antioxidant, a lubricant, and an anti-ultraviolet agent.
[0014] The preparation method of the low dielectric LCP composite material of the present invention comprises the following steps: mixing the components uniformly according to the proportion, extruding and granulating through a twin-screw extruder, with the screw barrel temperature ranging from 300 to 330° C., to obtain the low dielectric LCP composite material.
[0015] The present invention has the following beneficial effects: The present invention first prepares the low dielectric material through a process sequence of specific mixed acid (including HF, HCl and H2SO4) treatment and then calcination, and can obtain the low dielectric material with specific functional parameters, can effectively provide additional external and internal pores, thereby introducing air, and at the same time reduce the content of magnesium / aluminum elements, can effectively improve the dielectric properties of LCP resin, and make it have better comprehensive mechanical properties. DETAILED DESCRIPTION
[0016] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0017] The sources of raw materials used in the present invention are as follows: Sepiolite, palygorskite, diatomite and zeolite were purchased from Shou County, Henan Province.
[0018] LCP resin: purchased from Synanix, USA, D k =3.21, dielectric loss Tanδ is 0.0015, tensile strength is 88.03MPa, bending strength is 111.56MPa, impact strength is 66.02kJ / m 2 .
[0019] Glass fiber was purchased from Weifang, Shandong; Sericite was purchased from: Nanning, Guangxi; Hollow glass microspheres: Zhengzhou Saint-Laite.
[0020] The modification method of sepiolite is as follows: the sepiolite raw material is immersed in a mixed acid (A1: HF / H2SO4 / HCl=1:1:8; A2: HF / H2SO4 / HCl=2:7:1; B1: HF / H2SO4 / HCl=0:5:5; B2: HF / H2SO4 / HCl=1:9:0; B3: HF / H2SO4 / HCl=1:0:9; B4: HF) with a concentration of (A1: 1.0M; A2: 0.6M; B1: 1.0M; B2: 1.0M; B3: HF / H2SO4 / HCl=1:0:9; B4: HF), stirred at 40-60°C for 5-6 hours; washed with distilled water, and then dried; calcined the dried mineral raw material at 800-1000°C for 5-7 hours; and ground and screened to obtain low dielectric sepiolite.
[0021] Table 1: Filler parameters used in Examples and Comparative Examples Meerschaum Low dielectric sepiolite A1 Low dielectric sepiolite A2 Low dielectric sepiolite B1 Low dielectric sepiolite B2 Low dielectric sepiolite B3 Low dielectric sepiolite B4 <![CDATA[Specific surface area (m ^2 / g)]]> 155.26 267.26 192.21 170.23 235.79 187.26 138.80 Pore volume (cc / g) 0.47 0.92 0.76 0.65 0.84 0.52 0.31 Pore size (nm) 5.30 12.17 9.72 5.79 7.16 5.17 3.89 Al oxide (%) 6.58 1.15 0.77 2.03 2.78 3.46 1.21 Mg oxide (%) 19.9 2.06 2.23 5.66 4.07 2.60 1.71 Particle size (mesh) 800 800 800 800 800 800 1000 <![CDATA[D k ]]> 3.55 2.42 2.64 3.09 3.17 3.01 3.12 Tanδ 0.06 0.0021 0.0047 0.0089 0.0097 0.0074 0.0095 From the results in the above table, it can be seen that the mixed acid of the present application can effectively remove magnesium and aluminum oxides while expanding the pore structure. However, pure HF will seriously corrode silica, destroy the pore structure, cause the structure to collapse, and reduce the specific surface area, pore volume, and pore diameter.
[0022] The modification method of palygorskite is as follows: the palygorskite raw material is soaked in a mixed acid (A1: HF / H2SO4 / HCl=2:7:1; A2: HF / H2SO4 / HCl=1:2:2; B1: HF / H2SO4 / HCl=0:5:5; B2: HF / H2SO4 / HCl=1:9:0; B3: HF / H2SO4 / HCl=1:0:9; B4: HF) with a concentration of (A1: 0.8M; A2: 0.9M; B1: 0.8M; B2: 0.8M; B3: HF / H2SO4 / HCl=1:0:9; B4: HF), stirred at 40-60°C for 4-5 hours; washed with distilled water and then dried; calcined the dried mineral raw material at 800-1000°C for 6-8 hours; and low dielectric palygorskite is obtained after grinding and screening.
[0023] Table 1 continued: Palygorskite Low dielectric palygorskite A1 Low dielectric palygorskite A2 Low dielectric palygorskite B1 Low dielectric palygorskite B2 Low dielectric palygorskite B3 Low dielectric palygorskite B4 <![CDATA[Specific surface area (m ^2 / g)]]> 180.80 245.76 305.67 214.22 191.56 212.33 167.24 Pore volume (cc / g) 0.60 0.82 0.97 0.70 0.72 0.64 0.43 Pore size (nm) 6.7 9.24 14.14 7.97 7.21 7.02 5.49 Al oxide (%) 11.35 2.07 1.56 4.65 2.46 6.99 1.88 Mg oxide (%) 10.27 0.64 1.01 3.51 7.89 1.88 0.86 Particle size (mesh) 800 800 800 800 800 800 1000 <![CDATA[D k ]]> 3.72 2.53 2.48 2.97 3.13 3.01 3.14 Tanδ 0.040 0.0034 0.0025 0.0053 0.0080 0.0074 0.0091 The modification method of diatomite is as follows: soak the mineral raw material in a mixed acid (HF:HCl:H2SO4=0.5:1.5:8) with a concentration of (A1:1.0 M; A2:0.5 M), and stir at 40-60°C for 7 hours; wash with distilled water, and then dry; calcine the dried mineral raw material at 800-1000°C for 8 hours; and obtain low dielectric diatomite after grinding and screening.
[0024] Table 1 continued: diatomite Low dielectric diatomaceous earth A1 Low dielectric diatomaceous earth A2 <![CDATA[Specific surface area (m ^2 / g)]]> 62.87 170.55 102.33 Pore volume (cc / g) 0.046 0.097 0.066 Pore size (nm) 9.85 15.00 11.04 Al oxide (%) 1.44 0.33 0.84 Mg oxide (%) 0.19 0 0 Particle size (mesh) 800 800 800 <![CDATA[D k ]]> 3.27 2.48 2.86 Tanδ 0.024 0.0021 0.0027 The modification method of zeolite is as follows: soak the mineral raw material in a mixed acid of 0.6M concentration (A1: HF: HCl: H2SO4 = 1:1:8; A2: HF: HCl: H2SO4 = 1:2:3), and stir at 40-60°C for 6.5 hours; wash with distilled water, and then dry; calcine the dried mineral raw material at 800-1000°C for 8 hours; and obtain low dielectric zeolite after grinding and screening.
[0025] Zeolite Low dielectric zeolite A1 Low dielectric zeolite A2 <![CDATA[Specific surface area (m ^2 / g)]]> 68.89 195.47 155.89 Pore volume (cc / g) 0.16 0.78 0.54 Pore size (nm) 4.59 9.77 6.42 Al oxide (%) 5.62 2.78 3.22 Mg oxide (%) 0.43 0.011 0.028 Particle size (mesh) 800 800 800 <![CDATA[D k ]]> 4.1 2.43 2.76 Tanδ 0.048 0.0023 0.0033 Various test methods: (1) Dielectric properties of powders: The dielectric properties of powder samples at frequencies of 1 to 8 GHz were tested using the coaxial method using a 3656B vector network analyzer from China Electronics Co., Ltd. The sample and paraffin were mixed in a mass ratio of 5:5 and pressed into a ring with a thickness of about 3.2 mm.
[0026] (2) The dielectric properties of the composite LCP were tested using the waveguide method. According to the different proportions in the example, the resin was pressed into blocks of 47.3*22.2*2mm.
[0027] Preparation method of LCP composite material: According to the proportion, each component (LCP resin 70 parts, low dielectric filler or filler before modification and hollow glass microspheres 10 parts, glass fiber 15 parts, sericite 5 parts) was mixed evenly, and extruded into granules by a twin-screw extruder, and the screw barrel temperature was set to 320 o C~350 o C, and obtain a low dielectric LCP composite material.
[0028] Table 2: Test results of low dielectric LCP composite resins of the examples Example 1 Example 2 Comparative Example 1 Low dielectric filler Low dielectric sepiolite A1 Low dielectric sepiolite A2 Unmodified Sepiolite <![CDATA[D k ]]> 2.71 2.93 3.42 Tanδ 0.0022 0.0029 0.0093 Tensile strength / MPa 115.49 116.91 121.47 Bending strength / MPa 121.31 127.63 133.11 <![CDATA[Impact strength KJ / m 2 > 57.32 50.22 33.05 Table 2 continued: Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Low dielectric filler Low dielectric sepiolite B1 Low dielectric sepiolite B2 Low dielectric sepiolite B3 Low dielectric sepiolite B4 <![CDATA[D k ]]> 3.16 3.01 3.13 3.07 Tanδ 0.0035 0.0034 0.0042 0.0033 Tensile strength / MPa 113.63 110.17 95.44 115.33 Bending strength / MPa 122.34 115.67 110.54 114.43 <![CDATA[Impact strength KJ / m 2 > 46.66 50.03 20.35 43.12 Table 2 continued: Example 3 Example 4 Comparative Example 6 Low dielectric filler Low dielectric palygorskite A1 Low dielectric palygorskite A2 Unmodified palygorskite <![CDATA[D k ]]> 2.71 2.65 3.46 Tanδ 0.0032 0.0024 0.0098 Tensile strength / MPa 93.85 96.77 117.96 Bending strength / MPa 114.32 126.22 106.43 <![CDATA[Impact strength KJ / m 2 > 52.11 48.67 33.63 Table 2 continued: Comparative Example 7 Comparative Example 8 Comparative Example 9 Comparative Example 10 Low dielectric filler Low dielectric palygorskite B1 Low dielectric palygorskite B2 Low dielectric palygorskite B3 Low dielectric palygorskite B4 <![CDATA[D k ]]> 2.92 3.13 2.96 3.18 Tanδ 0.0032 0.0037 0.0031 0.0036 Tensile strength / MPa 95.33 98.62 86.78 100.13 Bending strength / MPa 120.31 116.42 90.44 114.65 <![CDATA[Impact strength KJ / m 2 > 46.89 48.91 28.26 39.68 Table 2 continued: Example 5 Example 6 Comparative Example 11 Low dielectric filler Low dielectric diatomaceous earth A1 Low dielectric diatomaceous earth A2 Unmodified diatomaceous earth <![CDATA[D k ]]> 2.68 2.89 3.07 Tanδ 0.0022 0.0024 0.0052 Tensile strength / MPa 101.36 103.96 119.36 Bending strength / MPa 107.69 115.52 112.02 <![CDATA[Impact strength KJ / m 2 > 84.76 76.76 64.76 Table 2 continued: Example 7 Example 8 Comparative Example 12 Comparative Example 9 Low dielectric filler Low dielectric zeolite A1 Low dielectric zeolite A2 Unmodified zeolite Hollow glass microspheres <![CDATA[D k ]]> 2.68 2.89 3.57 2.73 Tanδ 0.0023 0.0037 0.0074 0.0021 Tensile strength / MPa 101.22 94.88 92.63 120.11 Bending strength / MPa 121.63 113.38 111.32 118.41 <