Carbon dioxide-based biodegradable foam material and preparation method thereof
By using carbon dioxide foaming and combining specific components, a high-expansion, dimensionally stable carbon dioxide-based biodegradable foam material was prepared, solving the problems of high shrinkage and difficulty in molding in existing technologies, and realizing the application of environmentally friendly and efficient packaging materials.
Patent Information
- Application Number
- CN202411221558.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-22
AI Technical Summary
Existing carbon dioxide-propylene oxide copolymer foam products suffer from problems such as high shrinkage rate, residual odor from chemical foaming agents, and difficulty in molding irregularly shaped parts, which limit their application in the packaging materials field.
Carbon dioxide-based biodegradable foam materials are prepared using a carbon dioxide foaming method. By combining polypropylene carbonate, polybutylene terephthalate, and polylactic acid resin in specific proportions with cellulose, chain extender, compatibilizer, anti-shrinkage agent, and stabilizer, and using multi-stage foaming technology, a network skeleton structure and physical cross-linking points are formed, thereby improving dimensional stability.
A biodegradable foam material with high expansion ratio, dimensional stability, and easy molding of irregular parts was prepared. It is suitable for packaging cushioning fillers and irregular parts, and the process is environmentally friendly and can be mass-produced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of foaming materials, and more specifically to a carbon dioxide-based biodegradable foam material and a preparation method thereof. Background Art
[0002] Polymer foam materials are widely used due to their excellent comprehensive properties such as light weight, heat insulation, sound insulation and noise reduction. However, with the widespread application of foam materials, the "white pollution" problem of waste plastics has become increasingly serious. The treatment of foam waste has become a major problem. The main methods of waste treatment are landfill, incineration and recycling. Landfill often occupies a large amount of land; incineration will produce a large amount of carbon dioxide and harmful compounds such as nitrogen, sulfur, phosphorus, halogens, etc., which contribute to the greenhouse effect and the formation of acid rain. The use of recycling methods is limited by the properties, technology and cost of polymer materials themselves. With the increasing attention paid to environmental protection in today's society, it is imperative to develop biodegradable foam materials, especially in the field of packaging materials to replace existing foam materials (such as polystyrene foam materials).
[0003] At present, the commercialization of biodegradable foam materials has made significant progress. Synbra has developed the world's first polylactic acid foam material (BioFoam), and BASF has launched the certified compostable closed-cell foam material ecovioEA particles. With the increasing demand for biodegradable foams, more and more biodegradable resin materials have attracted widespread attention. Among them, polymethyl ethylene carbonate (PPC) is a biodegradable resin material prepared with carbon dioxide (CO2) (31% to 50% by mass) as the basic raw material. The source of resin raw materials, CO2 fixation, and can alleviate the shortage of petrochemical raw materials; at the same time, it can effectively solve the environmental pollution problem caused by foam material waste. However, in the development of PPC foam materials, when only the eco-friendly resin is foamed, the foamed foam material is easy to shrink at room temperature and cannot maintain its original shape. Regarding the preparation of foaming materials, technicians in related fields have conducted a lot of research. For example, patent CN104024336A introduces thermoplastic resins such as polybutylene succinate (PBS), ethylene-vinyl acetate copolymer (EVA), polypropylene (PP), etc., and prepares high-rate expandable polypropylene carbonate through chain extension and cross-linking, but biodegradability cannot be guaranteed. Patent CN102796361A uses water as a foaming agent, selects montmorillonite, diatomaceous earth, cellulose, etc. as carriers, solves the problems of technical production process safety and environmental protection, and prepares foam materials by extrusion foaming process, but does not give a specific product form; Patent CN109679307A introduces wheat straw powder as the main filler and vinyl silane as a cross-linking agent to form a cross-linked network structure to enhance foam elasticity, and prepares biodegradable pearl cotton sheets by extrusion foaming method. CN102796361A and CN109679307A are both prepared by extrusion process, and the product pore size is large, which affects the mechanical properties; the product needs to be cut when it is in sheet form, and it is difficult to prepare it into complex special-shaped structural parts. The PBAT / PPC foaming composite material invented by patent CN112662146A increases the melt strength of the system by adding PBAT / PPC with a suitable weight ratio, chain extender, and end-capping agent, and adopts a chemical foaming method to prepare a composite foaming material by extrusion foaming. The decomposition of chemical foaming agents often leads to residues that increase odor.
[0004] At present, pure PPC resin foaming is used to prepare foam products, which are easy to shrink and have poor dimensional stability, limiting its application in the field of packaging materials. Among the many measures taken to improve the dimensional stability of foam materials, there are still problems such as adding non-biodegradable resin modification, or using chemical foaming agents for foaming, residues increase odor, and the preparation process is difficult to prepare special-shaped parts in the form of foamed products, which seriously hinders the application and promotion of PPC foam materials. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a carbon dioxide-based biodegradable foam material and a preparation method thereof, which can solve the problems in the prior art such as large shrinkage rate of carbon dioxide-propylene oxide copolymer foaming products, residual odor of chemical foaming agents, and difficulty in molding and preparing special-shaped parts.
[0006] The present invention provides a carbon dioxide-based biodegradable foam material, which is prepared by foaming raw materials including the following components with carbon dioxide:
[0007] 100 parts by weight of biodegradable polymer;
[0008] 0.3-2.5 parts by weight of cellulose;
[0009] Chain extender 0.1~1.0 weight part;
[0010] Compatibilizer 0.3~1.0 parts by weight;
[0011] 1.0-2.5 parts by weight of anti-shrinkage agent;
[0012] Nucleating agent 0.3~1.0 weight part;
[0013] Stabilizer 0.1~0.5 parts by weight;
[0014] The biodegradable polymer is composed of polypropylene carbonate, polybutylene terephthalate-adipate and polylactic acid resin in a mass ratio of (70-25): (25-70): (1-5).
[0015] Preferably, the polypropylene carbonate is a carbon dioxide-propylene oxide copolymer, the polyether segment content is 4.5% to 15%, the number average molecular weight is 70 kg / mol to 180 kg / mol, and the molecular weight distribution is 2.0 to 3.5.
[0016] Preferably, the number average molecular weight of the polybutylene terephthalate-adipate is 40 kg / mol to 60 kg / mol, and the molecular weight distribution is 2.3 to 4.8.
[0017] Preferably, the polylactic acid resin includes polylactic acid and its copolymers; the polylactic acid is poly D-lactic acid and / or poly L-lactic acid, which is a crystalline polymer.
[0018] Preferably, the cellulose is cellulose nanofibers with a length of 1 μm to 5 μm;
[0019] The chain extender is an epoxy polymerization type chain extender with a molecular weight of 5000-10000 and an epoxy resin equivalent of 300 g / mol-500 g / mol;
[0020] The compatibilizer is maleic anhydride polyester;
[0021] The anti-shrinkage agent is distilled monoglyceride;
[0022] The nucleating agent is selected from one or more of talc, silicon dioxide, and zinc borate inorganic particles, and has a size of 1 μm to 5 μm.
[0023] The present invention also provides a method for preparing the carbon dioxide-based biodegradable foam material described in the above technical solution, comprising the following steps:
[0024] a) mixing a biodegradable polymer, cellulose, a chain extender, a compatibilizer, an anti-shrinkage agent, a nucleating agent and a stabilizer, and then melt-extruding and granulating to obtain resin particles;
[0025] b) foaming the resin particles obtained in step a) with CO2, and obtaining a carbon dioxide-based biodegradable foam material after stabilization treatment.
[0026] Preferably, the melt extrusion device in step a) is a twin-screw extruder, and the heating temperature is 150°C to 190°C.
[0027] Preferably, the aspect ratio of the granulation in step a) is (1-2):1, the length is 1 mm-2 mm, and the mass is 1 mg / granule-3 mg / granule.
[0028] Preferably, the foaming process in step b) is specifically as follows:
[0029] Add resin particles, water and isolation agent into a high-pressure resistant closed container, stir and disperse evenly, introduce CO2, the saturation pressure is 5MPa~15MPa, the saturation temperature is 60℃~110℃, the saturation time is 0.5h~2h, and then release the pressure at a pressure relief rate of 10MPa / s~20MPa / s to obtain 5~20 times of primary carbon dioxide-based plastic foamed particles; keep at 20℃~30℃ for 20h~30h, and the foamed particles will shrink to 5~17 times.
[0030] Preferably, the stabilization process in step b) is specifically as follows:
[0031] Air is introduced to maintain the pressure at 0.2MPa~0.5MPa, and the foamed particles are balanced under high pressure for 10h~20h, and then under hot steam at 80℃~120℃ for 10s~90s to obtain a dimensionally stable carbon dioxide-based biodegradable foam material that is 5 times~40 times larger.
[0032] The invention provides a carbon dioxide-based biodegradable foam material, which is prepared by foaming raw materials including the following components through carbon dioxide: 100 parts by weight of a biodegradable polymer; 0.3-2.5 parts by weight of cellulose; 0.1-1.0 parts by weight of a chain extender; 0.3-1.0 parts by weight of a compatibilizer; 1.0-2.5 parts by weight of an anti-shrinkage agent; 0.3-1.0 parts by weight of a nucleating agent; and 0.1-0.5 parts by weight of a stabilizer; the biodegradable polymer is composed of polypropylene carbonate, polybutylene terephthalate-adipate, and polylactic acid resin in a mass ratio of (70-25): (25-70): (1-5). Compared with the prior art, the carbon dioxide-based biodegradable foam material provided by the invention adopts specific content components to achieve better overall interaction, and the product has stable size, high multiple, and is easy to form special-shaped parts, and can be used as a cushioning packaging material or a packaging filler; and the added substances are all biodegradable, so that the obtained foam plastic has biodegradable characteristics.
[0033] In addition, the preparation method provided by the present invention has a simple process, does not use an organic foaming agent, is safe and environmentally friendly, can achieve large-scale production, and has broad application prospects. DETAILED DESCRIPTION
[0034] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The present invention provides a carbon dioxide-based biodegradable foam material, which is prepared by foaming raw materials including the following components with carbon dioxide:
[0036] 100 parts by weight of biodegradable polymer;
[0037] 0.3-2.5 parts by weight of cellulose;
[0038] Chain extender 0.1~1.0 weight part;
[0039] Compatibilizer 0.3~1.0 parts by weight;
[0040] 1.0-2.5 parts by weight of anti-shrinkage agent;
[0041] Nucleating agent 0.3~1.0 weight part;
[0042] Stabilizer 0.1~0.5 parts by weight;
[0043] The biodegradable polymer is composed of polypropylene carbonate, polybutylene terephthalate-adipate and polylactic acid resin in a mass ratio of (70-25): (25-70): (1-5).
[0044] The present invention provides a carbon dioxide-based biodegradable foam material, specifically a biodegradable carbon dioxide-propylene oxide copolymer foam plastic that is environmentally friendly, odorless, has a high magnification, and can be easily molded into special-shaped parts. The foam plastic is used to solve the problems in the prior art of large shrinkage of carbon dioxide-propylene oxide copolymer foamed products, odor generated by chemical foaming agents, and difficulty in molding and preparing special-shaped parts.
[0045] In the present invention, the carbon dioxide-based biodegradable foam material is prepared by carbon dioxide foaming of raw materials including biodegradable polymers, cellulose, chain extenders, compatibilizers, anti-shrinkage agents, nucleating agents and stabilizers, and foamed particles with a size of 5 to 40 times can be prepared by carbon dioxide foaming.
[0046] In the present invention, the biodegradable polymer is composed of polypropylene carbonate (PPC), polybutylene terephthalate-adipate (PBAT) and polylactic acid resin (PLA) in a mass ratio of (70-25): (25-70): (1-5). The present invention has no particular restrictions on the sources of the polypropylene carbonate (PPC), polybutylene terephthalate-adipate (PBAT) and polylactic acid resin (PLA), and commercially available products or self-made products of the above-mentioned biodegradable polymers well known to those skilled in the art can be used.
[0047] In a preferred embodiment of the present invention, the mass ratio of polypropylene carbonate (PPC), polybutylene terephthalate-adipate (PBAT) and polylactic acid (PLA) resin is 70:29:1, 50:48:2, 30:66:4, 60:37:3 or 25:70:5.
[0048] In the present invention, the polypropylene carbonate is preferably a carbon dioxide-propylene oxide copolymer, the polyether segment content is preferably 4.5% to 15% in molar ratio, the number average molecular weight is preferably 70kg / mol to 180kg / mol, and the molecular weight distribution is preferably 2.0 to 3.5. The polyether segment in the PPC molecular chain is conducive to ensuring the heat resistance, specific molecular weight and molecular weight distribution of the carbon dioxide-propylene oxide copolymer, and ensuring excellent comprehensive mechanical and thermal properties of the material.
[0049] In the present invention, the number average molecular weight of the polybutylene terephthalate-adipate is preferably 40 kg / mol to 60 kg / mol, and the molecular weight distribution is preferably 2.3 to 4.8.
[0050] In the present invention, the polylactic acid resin preferably includes polylactic acid and its copolymers, and more preferably polylactic acid; the polylactic acid is preferably poly D-lactic acid and / or poly L-lactic acid, which is a crystalline polymer.
[0051] The present invention has no special restrictions on the sources of the cellulose, compatibilizer, anti-shrinkage agent, nucleating agent and stabilizer, and commercially available products known to those skilled in the art may be used.
[0052] In the present invention, the cellulose is preferably cellulose nanofibers, and the length is preferably 1 μm to 5 μm, more preferably 2 μm to 3 μm.
[0053] In the present invention, the chain extender is preferably an epoxy polymerization type chain extender with a molecular weight (M w ) is preferably 5000~10000, and the epoxy resin equivalent is preferably 300g / mol~500g / mol; its synthetic monomers include glycidyl methacrylate (GMA), styrene, methyl methacrylate and cyclohexyl acrylate, etc. The chain extender can be synthesized by itself or purchased from commercial products, such as BASF's ADR series epoxy chain extenders.
[0054] In the present invention, the compatibilizer is preferably maleic anhydride polyester; the anti-shrinkage agent is preferably distilled monoglyceride; the nucleating agent is preferably selected from one or more of talc, silica, and zinc borate inorganic particles, more preferably talc; the size of the nucleating agent is preferably 1μm~5μm.
[0055] The invention provides a biodegradable carbon dioxide-propylene oxide copolymer foam material. The carbon dioxide-propylene oxide copolymer is used as a raw material and is blended with PBAT to improve the composite mechanical properties of the material. A network skeleton structure formed by a small amount of nanocellulose and the crystallization characteristics of polylactic acid (PLA) are used to form physical crosslinking points to enhance the ability of foam cell shaping. The multi-stage foaming technology is further combined to reduce the internal and external differences of the foam cell wall to improve the dimensional stability of the foamed product, so as to prepare high-ratio carbon dioxide-propylene oxide copolymer foamed particles.
[0056] The present invention also provides a method for preparing the carbon dioxide-based biodegradable foam material described in the above technical solution, comprising the following steps:
[0057] a) mixing a biodegradable polymer, cellulose, a chain extender, a compatibilizer, an anti-shrinkage agent, a nucleating agent and a stabilizer, and then melt-extruding and granulating to obtain resin particles;
[0058] b) foaming the resin particles obtained in step a) with CO2, and obtaining a carbon dioxide-based biodegradable foam material after stabilization treatment.
[0059] The invention firstly mixes biodegradable polymer, cellulose, chain extender, compatibilizer, anti-shrinkage agent, nucleating agent and stabilizer, and then performs melt extrusion and granulation to obtain resin particles.
[0060] In the present invention, the biodegradable polymer, cellulose, chain extender, compatibilizer, anti-shrinkage agent, nucleating agent and stabilizer are the same as those described in the above technical solution, and will not be described in detail here.
[0061] In the present invention, the mixing process preferably uses a high-speed mixer to achieve the purpose of mixing the raw materials uniformly.
[0062] In the present invention, the melt extrusion device is preferably a twin-screw extruder, and the heating temperature is preferably 150° C. to 190° C. After melt extrusion, the resin particles are preferably prepared by a dual-frequency pelletizer.
[0063] In the present invention, the aspect ratio of the granulation is preferably (1~2): 1, the length is preferably 1mm~2mm, and the mass is preferably 1mg / particle~3mg / particle; the resin particles of the above specifications obtained by granulation of the present invention are beneficial to the foaming of the particles.
[0064] After obtaining the resin particles, the present invention uses CO2 to foam the obtained resin particles, and obtains a carbon dioxide-based biodegradable foam material after stabilization treatment.
[0065] In the present invention, the foaming process is preferably specifically as follows:
[0066] Add resin particles, water and isolation agent into a high-pressure resistant closed container, stir and disperse evenly, introduce CO2, the saturation pressure is 5MPa~15MPa, the saturation temperature is 60℃~110℃, the saturation time is 0.5h~2h, and then release the pressure at a pressure relief rate of 10MPa / s~20MPa / s to obtain 5~20 times of primary carbon dioxide-based plastic foamed particles; keep at 20℃~30℃ for 20h~30h, and the foamed particles will shrink to 5~17 times.
[0067] The present invention has no special limitation on the type of the high-pressure resistant sealed container, and a high-pressure reaction kettle or a high-pressure resistant mold cavity well known to those skilled in the art can be used.
[0068] In the present invention, the stabilization process is preferably specifically as follows:
[0069] Air is introduced to maintain the pressure at 0.2MPa~0.5MPa, and the foamed particles are balanced under high pressure for 10h~20h, and then under hot steam at 80℃~120℃ for 10s~90s to obtain a dimensionally stable carbon dioxide-based biodegradable foam material that is 5 times~40 times larger.
[0070] In the present invention, the obtained dimensionally stable 5 to 40 times carbon dioxide-based biodegradable foam material can be directly used as a packaging cushioning filler or molded into a product for use in the packaging field.
[0071] The present invention places the obtained resin particles in a high pressure container, and then fills the high pressure container with carbon dioxide, heats the high pressure container to the foaming temperature, and keeps the pressure at a constant temperature for a certain time. After the resin particles absorb carbon dioxide, they are subjected to pressure relief treatment, and carbon dioxide-propylene oxide copolymer foam plastics are obtained after cooling; the present invention processes by pressure relief, so that the carbon dioxide in the resin particles is driven by the internal and external pressure difference, and spontaneous nucleation growth, and then the resin particles are foamed to obtain carbon dioxide-based copolymer foam particles. Afterwards, air is introduced, and the pressure is slowly increased, wherein the pressure-increasing process of slowly increasing the pressure is adopted, and the primary carbon dioxide-based copolymer foam particles can be prevented from being flattened and deformed, and the expansion process is affected. The pressure-increasing rate is preferably 0.02MPa / h~0.05MPa / h, and the storage tank particles are discharged after hot steam is introduced for a certain time, and the carbon dioxide-based copolymer foam particles are softened because the melt is melted by heat, and the driving force of the internal pressure causes the primary carbon dioxide-based copolymer foam particles to restore their shape and further expand.
[0072] In the present invention, the prepared 5-40 times carbon dioxide-based biodegradable foamed particles can be pre-pressed and can be formed into special-shaped parts through conventional EPP and EPS molding machine equipment and steam molds. The products can be widely used in the packaging field; in addition, the carbon dioxide-based biodegradable foam material can also be directly used as a cushioning filler.
[0073] The preparation method provided by the invention has simple process, does not use organic foaming agent, has safe process, is environmentally friendly, can realize large-scale production, and has broad application prospects.
[0074] The invention provides a carbon dioxide-based biodegradable foam material, which is prepared by foaming raw materials including the following components through carbon dioxide: 100 parts by weight of a biodegradable polymer; 0.3-2.5 parts by weight of cellulose; 0.1-1.0 parts by weight of a chain extender; 0.3-1.0 parts by weight of a compatibilizer; 1.0-2.5 parts by weight of an anti-shrinkage agent; 0.3-1.0 parts by weight of a nucleating agent; and 0.1-0.5 parts by weight of a stabilizer; the biodegradable polymer is composed of polypropylene carbonate, polybutylene terephthalate-adipate and polylactic acid resin in a mass ratio of (70-25): (25-70): (1-5). Compared with the prior art, the carbon dioxide-based biodegradable foam material provided by the invention adopts specific content components to achieve overall good interaction, the product has stable size, high multiple, easy to form special-shaped parts, and can be used as a cushioning packaging material or packaging filler; and the added substances are all biodegradable, so that the obtained carbon dioxide-propylene oxide copolymer foam plastic has biodegradable characteristics.
[0075] In addition, the preparation method provided by the present invention has a simple process, does not use an organic foaming agent, is safe and environmentally friendly, can achieve large-scale production, and has broad application prospects.
[0076] To further illustrate the present invention, the following examples are used to provide a detailed description. The polypropylene carbonate (PPC) HF-901 used in the present invention was purchased from Zhejiang Huafeng Environmental Protection Materials Co., Ltd.; the polybutylene adipate terephthalate (PBAT) HF101 used was provided by Huafeng Group Co., Ltd.; polylactic acid (PLA) REVODE190 was a product of Zhejiang Haizheng Biomaterial Co., Ltd.; cellulose 2μm was provided by Northern Century (Jiangsu) Cellulose Materials Co., Ltd.; compatibilizer CYD-190A was provided by Weihai Chenyuan Molecular New Materials Co., Ltd.; chain extender ADR-4468 was provided by BASF SE; nucleating agent talc powder with a specification of 5000 mesh was provided by Haicheng Hetai Powder Technology Co., Ltd.; anti-shrinkage monoglyceride DMG-95 was provided by Hangzhou Fuchun Food Additives Co., Ltd.; stabilizer GN01 was provided by Changchun Xinshunda Packaging Co., Ltd.
[0077] The present invention will be described below according to the embodiments and comparative examples, but the present invention is not limited to these embodiments. In addition, when not specifically stated, "parts" and "%" are all weight standards. In addition, the evaluation in the embodiments and comparative examples is carried out according to the following method.
[0078] The measuring volume is about 100cm 3 After the weight w (g) of the PPC resin pre-expanded particles, the volume increase (immersion volume) v (cm 3), and according to the density d(g / cm 3 ), the expansion ratio was calculated using the formula: expansion ratio = d × v / w.
[0079] Comparative Example 1
[0080] Weigh each material according to the resin formula: 100 parts by weight of polypropylene carbonate, 0.5 parts by weight of nucleating agent talc, 0.2 parts by weight of stabilizer, mix PPC, nucleating agent and stabilizer evenly through a high mixer, and control the heating temperature of each section of the extruder in the range of 150-190°C. After the resin is melt-extruded through a twin-screw extruder, PPC resin particles are prepared through a dual-frequency pelletizer, with a particle size L / D of 1-2, a particle length L controlled at 1-2mm, and a controlled mass of 2mg / particle.
[0081] Then, 800g of PPC resin particles, 1600g of deionized water, and 3g of talcum powder, an isolating agent, were added to a 3L high-pressure sealed container, and stirred at a speed of 400r / min to disperse evenly. CO2 was introduced into the high-pressure sealed container, with a saturation pressure of 5.5MPa, a saturation temperature of 60°C, and a saturation time of 1.5h. The pressure of the autoclave was released at a pressure relief rate of 15MPa / s to obtain 20 times primary carbon dioxide-based copolymer plastic foamed particles. The temperature (25°C) was maintained for 24h, and the foamed particles were shrunk to 5 times.
[0082] Example 1
[0083] Weigh each material according to the resin formula: 70 parts by weight of polypropylene carbonate (PPC), 29 parts by weight of butylene adipate terephthalate (PBAT), 1.0 parts by weight of polylactic acid, 0.3 parts by weight of cellulose, 0.7 parts by weight of compatibilizer, 0.15 parts by weight of chain extender, 1.5 parts by weight of anti-shrinkage agent, 0.5 parts by weight of nucleating agent talc, 0.2 parts by weight of stabilizer, mix PPC, PBAT, polylactic acid, cellulose, compatibilizer, chain extender, anti-shrinkage agent, nucleating agent and stabilizer evenly through a high mixer, and control the heating temperature of each section of the extruder in the range of 150~190℃. After the resin is melt-extruded in a twin-screw extruder, PPC resin particles are prepared by a dual-frequency pelletizer, and the particle size L / D is 1~2, the particle length L is controlled at 1~2mm, and the mass is controlled at 2mg / particle.
[0084] Then, 800g of PPC resin particles, 1600g of deionized water, and 3g of talcum powder, an isolating agent, were added to a 3L high-pressure sealed container, and stirred at a speed of 400r / min to disperse evenly. CO2 was introduced into the high-pressure sealed container, with a saturation pressure of 6.2MPa, a saturation temperature of 75°C, and a saturation time of 1.5h. The pressure of the autoclave was released at a pressure relief rate of 15MPa / s to obtain 8-fold primary carbon dioxide-based copolymer plastic foamed particles. The temperature (25°C) was maintained for 24h, and the foamed particles shrunk to 7 times.
[0085] The carbon dioxide-based copolymer plastic foam particles were placed in a closed storage tank, and air was introduced to maintain the pressure at 0.2 MPa. The foamed particles were balanced under high pressure for 16 hours. After the particles in the storage tank were unloaded, 80°C hot air was introduced for 15 seconds to obtain dimensionally stable 8-fold foamed particles (tested after 24 hours).
[0086] Example 2
[0087] Weigh each material according to the resin formula: 50 parts by weight of polypropylene carbonate (PPC), 48 parts by weight of butylene adipate terephthalate (PBAT), 2 parts by weight of polylactic acid, 0.7 parts by weight of cellulose, 0.7 parts by weight of compatibilizer, 0.15 parts by weight of chain extender, 1.5 parts by weight of anti-shrinkage agent, 0.5 parts by weight of nucleating agent talc, 0.2 parts by weight of stabilizer, mix PPC, PBAT, PLA, cellulose, compatibilizer, chain extender, anti-shrinkage agent, nucleating agent and stabilizer evenly through a high mixer, and control the heating temperature of each section of the extruder in the range of 150~190℃. After the resin is melt-extruded in a twin-screw extruder, PPC resin particles are prepared by a dual-frequency pelletizer, and the particle size L / D is 1~2, the particle length L is controlled at 1~2mm, and the mass is controlled at 2mg / particle.
[0088] Then, 800g of PPC resin particles, 1600g of deionized water, and 3g of talcum powder, an isolating agent, were added to a 3L high-pressure sealed container, and stirred at a speed of 400r / min to disperse evenly. CO2 was introduced into the high-pressure sealed container, with a saturation pressure of 8.5MPa, a saturation temperature of 95°C, and a saturation time of 1.5h. The pressure of the autoclave was released at a pressure relief rate of 15MPa / s to obtain 15-fold primary carbon dioxide-based copolymer plastic foamed particles. The temperature (25°C) was maintained for 24h, and the foamed particles were shrunk to 12 times.
[0089] The carbon dioxide-based copolymer plastic foam particles were placed in a closed storage tank, and air was introduced to maintain the pressure at 0.2 MPa. The foamed particles were balanced under high pressure for 16 hours. After the particles in the storage tank were unloaded, 95°C hot air was introduced for 20 seconds to obtain dimensionally stable 16-fold foamed particles (tested after 24 hours).
[0090] Example 3
[0091] Weigh each material according to the resin formula: 30 parts by weight of polypropylene carbonate (PPC), 66 parts by weight of butylene adipate terephthalate (PBAT), 4 parts by weight of polylactic acid, 1.5 parts by weight of cellulose, 0.7 parts by weight of compatibilizer, 0.15 parts by weight of chain extender, 1.5 parts by weight of anti-shrinkage agent, 0.5 parts by weight of nucleating agent talc, 0.2 parts by weight of stabilizer, mix PPC, PBAT, PLA, cellulose, compatibilizer, chain extender, anti-shrinkage agent, nucleating agent and stabilizer evenly through a high mixer, and control the heating temperature of each section of the extruder in the range of 150~190℃. After the resin is melt-extruded in a twin-screw extruder, PPC resin particles are prepared by a dual-frequency pelletizer, and the particle size L / D is 1~2, the particle length L is controlled at 1~2mm, and the mass is controlled at 2mg / particle.
[0092] Then, 800g of PPC resin particles, 1600g of deionized water, and 3g of talcum powder, an isolating agent, were added to a 3L high-pressure sealed container, and stirred at a speed of 400r / min to disperse evenly. CO2 was introduced into the high-pressure sealed container, with a saturation pressure of 9.5MPa, a saturation temperature of 105°C, and a saturation time of 1.5h. The pressure of the autoclave was released at a pressure relief rate of 15MPa / s to obtain 25 times primary carbon dioxide-based copolymer plastic foamed particles. The temperature (25°C) was maintained for 24h, and the foamed particles were shrunk to 15 times.
[0093] The carbon dioxide-based copolymer plastic foam particles were placed in a closed storage tank, and air was introduced to maintain the pressure at 0.5 MPa. The foam particles were balanced under high pressure for 16 hours. After the particles in the storage tank were unloaded, 110°C hot steam was introduced for 45 seconds to obtain dimensionally stable 40-fold foam particles (tested after 24 hours).
[0094] Example 4
[0095] Weigh each material according to the resin formula: 60 parts by weight of polypropylene carbonate (PPC), 37 parts by weight of butylene adipate terephthalate (PBAT), 3.0 parts by weight of polylactic acid, 2 parts by weight of cellulose, 0.7 parts by weight of compatibilizer, 0.15 parts by weight of chain extender, 1.5 parts by weight of anti-shrinkage agent, 0.5 parts by weight of nucleating agent talc, 0.2 parts by weight of stabilizer, mix PPC, PBAT, PLA, cellulose, compatibilizer, chain extender, anti-shrinkage agent, nucleating agent and stabilizer evenly through a high mixer, and control the heating temperature of each section of the extruder in the range of 150~190℃. After the resin is melt-extruded in a twin-screw extruder, PPC resin particles are prepared by a dual-frequency pelletizer, and the particle size L / D is 1~2, the particle length L is controlled at 1~2mm, and the mass is controlled at 2mg / particle.
[0096] Then, 800g of PPC resin particles, 1600g of deionized water, and 3g of talcum powder, an isolating agent, were added to a 3L high-pressure sealed container, and stirred at a speed of 400r / min to disperse evenly. CO2 was introduced into the high-pressure sealed container, with a saturation pressure of 7MPa, a saturation temperature of 67°C, and a saturation time of 1.5h. The pressure of the autoclave was released at a pressure relief rate of 15MPa / s to obtain 20 times primary carbon dioxide-based copolymer plastic foamed particles. The temperature (25°C) was maintained for 24h, and the foamed particles shrunk to 13 times.
[0097] The carbon dioxide-based copolymer plastic foam particles were placed in a closed storage tank, and air was introduced to maintain the pressure at 0.4 MPa. The foamed particles were balanced under high pressure for 16 hours. After the particles in the storage tank were unloaded, 80°C hot air was introduced for 50 seconds to obtain dimensionally stable 35-fold foamed particles (tested after 24 hours).
[0098] Example 5
[0099] Weigh each material according to the resin formula: 25 parts by weight of polypropylene carbonate (PPC), 70 parts by weight of butylene adipate terephthalate (PBAT), 5 parts by weight of polylactic acid, 0.5 parts by weight of cellulose, 0.7 parts by weight of compatibilizer, 0.15 parts by weight of chain extender, 1.5 parts by weight of anti-shrinkage agent, 0.5 parts by weight of nucleating agent talc, 0.2 parts by weight of stabilizer, mix PPC, PBAT, PLA, cellulose, compatibilizer, chain extender, anti-shrinkage agent, nucleating agent and stabilizer evenly through a high mixer, and control the heating temperature of each section of the extruder in the range of 150~190℃. After the resin is melt-extruded in a twin-screw extruder, PPC resin particles are prepared by a dual-frequency pelletizer, and the particle size L / D is 1~2, the particle length L is controlled at 1~2mm, and the mass is controlled at 2mg / particle.
[0100] Then, 800g of PPC resin particles, 1600g of deionized water, and 3g of talcum powder, an isolating agent, were added to a 3L high-pressure sealed container, and stirred at a speed of 400r / min to disperse evenly. CO2 was introduced into the high-pressure sealed container, with a saturation pressure of 13MPa, a saturation temperature of 107℃, and a saturation time of 1.5h. The pressure of the autoclave was released at a pressure relief rate of 15MPa / s to obtain 20 times primary carbon dioxide-based copolymer plastic foamed particles. The temperature (25℃) was maintained for 24h, and the foamed particles shrunk to 17 times.
[0101] The carbon dioxide-based copolymer plastic foam particles were placed in a closed storage tank, and air was introduced to maintain the pressure at 0.35 MPa. The foam particles were balanced under high pressure for 16 hours. After the particles in the storage tank were unloaded, 112°C hot steam was introduced for 37 seconds to obtain dimensionally stable 25-fold foam particles (tested after 24 hours).
[0102] Table 1 PPC foamed particles example formula and results
[0103]
[0104] As shown in Table 1, the foam formed in Comparative Example 1 had a foaming ratio of 20 times, and the foamed foam shrank within 24 hours at room temperature and could not maintain its shape. The foam formed in each of Examples 1 to 5 maintained a foaming ratio of 5 to 40 after 24 hours, and also showed excellent shape stability and dimensional stability.
[0105] In summary, the present invention provides a biodegradable carbon dioxide-propylene oxide copolymer foam material and a preparation method thereof, wherein carbon dioxide-propylene oxide copolymer is used as a raw material and blended with PBAT to improve the composite mechanical properties of the material; a network skeleton structure formed by a small amount of nanocellulose and the crystallization characteristics of polylactic acid (PLA) are used to form physical crosslinking points to enhance the ability of foam shaping; and multi-stage foaming technology is further combined to reduce the internal and external differences of the foam wall to improve the dimensional stability of the foamed product, and prepare high-ratio carbon dioxide-propylene oxide copolymer foamed particles. At the same time, the present invention does not use an organic foaming agent, the production process is safe and environmentally friendly, and large-scale production can be achieved. The obtained foamed particles are stable in size, high in multiples, and easy to form special-shaped parts, and the added substances are all biodegradable, so that the obtained carbon dioxide-propylene oxide copolymer foam plastic has biodegradable characteristics.
[0106] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A carbon dioxide-based biodegradable foam material, prepared by foaming the following raw materials with carbon dioxide: 100 parts by weight of biodegradable polymer; 0.3-2.5 parts by weight of cellulose; Chain extender 0.1~1.0 weight part; Compatibilizer 0.3~1.0 parts by weight; 1.0-2.5 parts by weight of anti-shrinkage agent; Nucleating agent 0.3~1.0 weight part; Stabilizer 0.1~0.5 parts by weight; The biodegradable polymer is composed of polypropylene carbonate, polybutylene terephthalate-adipate and polylactic acid resin in a mass ratio of (70-25): (25-70): (1-5).
2. The carbon dioxide-based biodegradable foam material according to claim 1, It is characterized in that The polypropylene carbonate is a carbon dioxide-propylene oxide copolymer, has a polyether segment content of 4.5% to 15%, a number average molecular weight of 70 kg / mol to 180 kg / mol, and a molecular weight distribution of 2.0 to 3.
5.
3. The carbon dioxide-based biodegradable foam material according to claim 1, It is characterized in that The number average molecular weight of the polybutylene terephthalate-adipate is 40 kg / mol to 60 kg / mol, and the molecular weight distribution is 2.3 to 4.
8.
4. The carbon dioxide-based biodegradable foam material according to claim 1, It is characterized in that The polylactic acid resin includes polylactic acid and its copolymer; the polylactic acid is poly D-lactic acid and / or poly L-lactic acid, which is a crystalline polymer.
5. The carbon dioxide-based biodegradable foam material according to claim 1, It is characterized in that The cellulose is cellulose nanofibers with a length of 1 μm to 5 μm; The chain extender is an epoxy polymerization type chain extender with a molecular weight of 5000-10000 and an epoxy resin equivalent of 300 g / mol-500 g / mol; The compatibilizer is maleic anhydride polyester; The anti-shrinkage agent is distilled monoglyceride; The nucleating agent is selected from one or more of talc, silicon dioxide, and zinc borate inorganic particles, and has a size of 1 μm to 5 μm.
6. A method for preparing the carbon dioxide-based biodegradable foam material according to any one of claims 1 to 5, The following steps are involved: a) mixing a biodegradable polymer, cellulose, a chain extender, a compatibilizer, an anti-shrinkage agent, a nucleating agent and a stabilizer, and then melt-extruding and granulating to obtain resin particles; b) Using CO 2 The resin particles obtained in step a) are foamed and stabilized to obtain a carbon dioxide-based biodegradable foam material.
7. The preparation method according to claim 6, It is characterized in that The melt extrusion device in step a) is a twin-screw extruder, and the heating temperature is 150°C to 190°C.
8. The preparation method according to claim 6, It is characterized in that The aspect ratio of the granulation in step a) is (1-2): 1, the length is 1 mm-2 mm, and the mass is 1 mg / granule-3 mg / granule.
9. The preparation method according to claim 6, It is characterized in that The foaming process in step b) is specifically as follows: Add resin particles, water and isolation agent into a high pressure sealed container, stir and disperse evenly, and introduce CO 2 The saturation pressure is 5MPa~15MPa, the saturation temperature is 60℃~110℃, the saturation time is 0.5h~2h, and then the pressure is released at a pressure relief rate of 10MPa / s~20MPa / s to obtain 5 times~20 times the primary carbon dioxide-based plastic foamed particles; keep it at 20℃~30℃ for 20h~30h, and the foamed particles shrink to 5 times~17 times.
10. The preparation method according to claim 6, It is characterized in that The stabilization process in step b) is specifically as follows: Air is introduced to maintain the pressure at 0.2MPa~0.5MPa, and the foamed particles are balanced under high pressure for 10h~20h, and then under hot steam at 80℃~120℃ for 10s~90s to obtain a dimensionally stable carbon dioxide-based biodegradable foam material that is 5 times~40 times larger.
Citation Information
Cited By
Environment-friendly air conditioner packaging foam and preparation method thereof
CN121045771A
Environment-friendly air conditioner packaging foam and preparation method thereof
CN121045771B