Surface treatment process for improving weather resistance of iron oxide pigment

Through nanomaterial coating technology, the problem of discoloration and fading of iron oxide pigments in humid environments is solved, which significantly improves its weather resistance and wear resistance and extends its service life.

CN118994940APending Publication Date: 2024-11-22YIXING YUXING IND & TRADE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411108456.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Iron oxide pigments are prone to discoloration and fading in humid environments, and have poor weather resistance, making them difficult to withstand climate tests outdoors, such as light aging, cold and cold, wind and rain corrosion.

Method used

Nanomaterials (such as nanosilica, nanozirconia and nanotitanium dioxide) are mixed with iron oxide pigment slurry, and the cladding layer is formed by self-assembly layered layers, and high-temperature stirring and roasting are used to form a stable The nano-clad layer improves the wear resistance and aging resistance of the pigment.

Benefits of technology

It significantly improves the weather resistance and wear resistance of iron oxide pigments, extends the service life of the pigments, while maintaining the stability and gloss of color.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994940A_ABST
    Figure CN118994940A_ABST
Patent Text Reader

Abstract

The invention discloses a surface treatment process for improving weather resistance of an iron oxide pigment, and belongs to the technical field of inorganic pigment surface functionalization treatment. The preparation method comprises the following steps: firstly, adding a nano material into slurry prepared from iron oxide red pigment, heating and stirring to obtain mixed slurry; adding an organic adhesive and a curing agent into the mixed slurry, stirring at high temperature, cooling, adding a dispersing agent, fully mixing to obtain a material, drying, roasting, cooling and grinding to obtain the surface-treated iron oxide red pigment. After the surface of the iron oxide pigment is treated, the weather resistance and the wear resistance of the iron oxide pigment are greatly improved, the application performance of the pigment is well improved, and great economic benefits and market application values are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface functionalization treatment of inorganic pigments, and in particular relates to a surface treatment process for improving the weather resistance of iron oxide pigments. Background Art

[0002] Iron oxide pigments that have been surface treated are pigments with good dispersibility, excellent light resistance and weather resistance. Iron oxide pigments mainly refer to four types of coloring pigments, namely iron oxide red, iron yellow, iron black and iron brown, which are based on iron oxide. Among them, iron oxide red is the main one (accounting for about 50% of iron oxide pigments). Mica iron oxide used as anti-rust pigments and magnetic iron oxide used as magnetic recording materials also belong to the category of iron oxide pigments. Iron oxide is the second largest inorganic pigment after titanium dioxide and the largest colored inorganic pigment. Among all the iron oxide pigments consumed, more than 70% are prepared by chemical synthesis, which is called synthetic iron oxide. Synthetic iron oxide has high synthetic purity, uniform particle size, wide color spectrum, multiple colors, low price, non-toxicity, excellent coloring and application performance, and has the properties of absorbing ultraviolet rays. Therefore, it is widely used in building materials, coatings, plastics, electronics, tobacco, medicine, rubber, ceramics, inks, magnetic materials, papermaking and other fields.

[0003] Weathering resistance generally refers to a series of aging phenomena such as fading, discoloration, cracking, chalking and strength loss of plastic products due to external conditions such as sunlight, temperature changes, wind and rain. Among them, ultraviolet radiation is the key factor that promotes plastic aging. The light resistance and weathering resistance of pigments are important indicators to measure the application performance of pigments. Weathering resistance is a term used to describe the various changes in the appearance and functional value of colored coatings. It covers comprehensive external use capabilities, such as color and gloss retention, chalking, adhesion and film integrity. The initial impact is caused by the degradation of organic binders exposed to sunlight, moisture, temperature changes and environmental pollution. Chalking is due to the separation of increasing organic binders from the surface of the paint film, leaving pigments and some extender particles exposed to the air, thus forming a powdery and chalky appearance. This change will lead to color changes and loss of gloss.

[0004] As a multi-color pigment, iron oxide has many characteristics that other pigments do not have, such as tinting power and oil absorption. In addition, iron oxide has a certain shielding effect on ultraviolet radiation, which can extend the application life of the coating. However, in order to achieve excellent weather resistance of the coating film, it must be chemically modified or surface treated. According to the different application environments of different coating systems, different methods are selected to improve the weather resistance of iron oxide pigments, which can effectively extend the service life of the pigments and maintain good color. Generally speaking, inorganic pigments will darken and deepen under the influence of sunlight and atmosphere, while organic pigments will mostly fade. In general, the light resistance and weather resistance of inorganic pigments are much stronger than those of general organic pigments. If the chemical stability of the pigment is poor, the chemical composition of the pigment will change under the influence of sunlight and atmosphere. Due to the change in chemical composition, the color will also change. For example, the darkening of zinc barium white in the sun is due to the reduction of zinc sulfide to metallic zinc.

[0005] In summary, how to use surface treatment technology to improve the weather resistance and wear resistance of iron oxide pigments so that iron oxide pigments can be used outdoors to withstand the test of climate, such as the comprehensive damage caused by light aging, cold and heat, wind and rain, bacteria and acid rain corrosion, has become a problem that needs to be solved urgently. Summary of the invention

[0006] In order to solve the technical problems that the above-mentioned iron oxide pigment has poor weather resistance and is easy to change color and fade in a humid environment, the purpose of the present invention is to provide a surface treatment process for iron oxide pigment to improve the weather resistance of iron oxide pigment and extend the service life of the pigment.

[0007] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0008] A surface treatment process for improving the weather resistance of an iron oxide pigment comprises adding a nano material to a slurry prepared with an iron oxide red pigment, heating and stirring to obtain a mixed slurry; then adding an organic adhesive and a curing agent to the mixed slurry, stirring at a high temperature, adding a dispersant after cooling, fully mixing to obtain a material, and drying, roasting, cooling, and grinding to obtain a surface-treated iron oxide red pigment.

[0009] Furthermore, the iron oxide red slurry is prepared by mixing and stirring the iron oxide red pigment and deionized water, and the concentration is 45-70%.

[0010] Furthermore, the nanomaterials are nano silicon dioxide, nano zirconium dioxide and nano titanium dioxide.

[0011] Furthermore, the ratio of the added nanomaterials is: silicon: zirconium: titanium: iron is 0.1-1.5:0.1-0.5:0.5-3:10.

[0012] Furthermore, the ratio of the added nanomaterials is: silicon: zirconium: titanium: iron is 1.5:0.5:3:10.

[0013] Furthermore, the organic adhesive is epoxy resin; and the curing agent is polyamide.

[0014] Furthermore, the high temperature stirring temperature is 140° C. to 160° C.; the stirring rate is 450 to 550 r / min.

[0015] Furthermore, the dispersant is an alcoholamine dispersant, selected from one or a combination of diethanolamine, triethanolamine, isopropanolamine, and N,N-dimethylethanolamine.

[0016] Furthermore, the proportion of the organic adhesive added in the mixed slurry is 5-25%; the proportion of the curing agent added in the mixed slurry is 2-8%.

[0017] Furthermore, any of the above-mentioned surface treatment processes for improving the weather resistance of iron oxide pigments comprises the following steps:

[0018] (1) mixing and stirring red iron oxide pigment and deionized water to prepare a slurry of 45-70%;

[0019] (2) adding nano silicon dioxide to the slurry of step (1) at a silicon-iron ratio of 0.1 to 1.5:10, adding nano zirconium oxide to the slurry of step (1) at a zirconium-iron ratio of 0.1 to 0.5:10, and adding nano titanium dioxide to the slurry of step (1) at a titanium-iron ratio of 0.5 to 3:10, heating to 60° C., stirring at 100 r / min for 15 min, and obtaining a mixed slurry;

[0020] (3) adding 5-25% of epoxy resin and 2-8% of polyamide to the mixed slurry obtained in step (2), and then continuing to heat to 145° C., stirring at a speed of 500 r / min for 50-120 min; after naturally cooling to room temperature, adding 0.5-1% of an alcohol amine dispersant, dispersing at high speed to fully mix, and obtaining a material;

[0021] (4) After drying the mixed material in step (3), the mixed material is introduced into a calcining furnace and calcined at a temperature of 250° C. to 300° C. for 5 to 8 hours under a nitrogen atmosphere. After naturally cooling to room temperature, the mixed material is ground to obtain a surface-treated iron oxide red pigment.

[0022] Beneficial effects: Compared with the prior art, the advantages of the present invention are as follows:

[0023] (1) The present invention uses nanomaterials (such as nano silicon dioxide, nano zirconium oxide and nano titanium dioxide) to preliminarily mix with iron oxide pigment slurry, so that the nanomaterials are covered on the surface of iron oxide particles through layer-by-layer self-assembly to form a coating layer, and uses organic resin and polyamide through appropriate heat treatment to make the nano coating layer and the iron oxide particles more firmly bonded, which can effectively improve the surface state of the iron oxide pigment and greatly improve the wear resistance and aging resistance of the iron oxide pigment without affecting the gloss and color.

[0024] (2) The nano-silicon dioxide and nano-titanium dioxide used in the present invention have high ultraviolet shielding performance and weather resistance. They are coated on the surface of iron oxide to reduce the area of ​​the iron oxide pigment exposed to the outside and in direct contact with the air, thereby effectively reducing the aging rate of the iron oxide pigment.

[0025] (3) In the present invention, nano-zirconium dioxide is added to the nano-silicon dioxide and nano-titanium dioxide when preparing the coating material. Since nano-zirconium dioxide has ultra-high strength and high toughness, it has excellent wear resistance after being composited with the pigment.

[0026] (4) The present invention strictly controls the amount of the added multiple nanomaterials and adds polyamide during the composite process, thereby reducing the surface activity of the nanomaterials and inhibiting the occurrence of agglomeration, so that the nanocomposite material can be effectively coated on the surface of the iron oxide pigment, thereby improving the aging resistance and wear resistance of the iron oxide pigment. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a picture of iron oxide red pigment coated with nanomaterials.

[0028] Figure 2 This is a picture of ordinary iron oxide red pigment without surface coating treatment. DETAILED DESCRIPTION

[0029] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with specific embodiments.

[0030] Unless otherwise specified, the reagents or drugs used in the following examples are commercially available products.

[0031] Example 1

[0032] A surface treatment process for iron oxide pigments, the steps are as follows:

[0033] (1) Pour the iron oxide red pigment and deionized water into a mixer, mix and stir to prepare a 45-70% slurry;

[0034] (2) adding nano silicon dioxide to the slurry of step (1) at a silicon-iron ratio of 0.1 to 1.5:10, adding nano zirconium oxide to the slurry of step (1) at a zirconium-iron ratio of 0.1 to 0.5:10, and adding nano titanium dioxide to the slurry of step (1) at a titanium-iron ratio of 0.5 to 3:10, heating to 60° C., stirring at 100 r / min for 15 min, and obtaining a mixed slurry;

[0035] (3) adding 5-25% of epoxy resin and 2-8% of polyamide to the mixed slurry obtained in step (2), and then continuing to heat to 145° C., stirring at a speed of 500 r / min for 50-120 min; after naturally cooling to room temperature, adding 0.5-1% of an alcohol amine dispersant (one or a combination of diethanolamine, triethanolamine, isopropanolamine, and N,N-dimethylethanolamine), and dispersing at high speed to fully mix the mixture to obtain a material;

[0036] (4) After drying the mixed material in step (3), the mixed material is introduced into a calcining furnace and calcined at a temperature of 250° C. to 300° C. for 5 to 8 hours under a nitrogen atmosphere. After naturally cooling to room temperature, the mixed material is ground to obtain a surface-treated iron oxide red pigment.

[0037] Example 2

[0038] A surface treatment process for iron oxide pigments, the steps are as follows:

[0039] (1) Pour the iron oxide red pigment and deionized water into a mixer, mix and stir to prepare a 45% slurry;

[0040] (2) adding nano silicon dioxide to the slurry of step (1) at a silicon-iron ratio of 1.5:10, adding nano zirconium oxide to the slurry of step (1) at a zirconium-iron ratio of 0.5:10, and adding nano titanium dioxide to the slurry of step (1) at a titanium-iron ratio of 3:10, heating to 60° C., stirring at 100 r / min for 15 min, and obtaining a mixed slurry;

[0041] (3) adding 15% of epoxy resin and 6% of polyamide to the mixed slurry obtained in step (2), and then continuing to heat to 145° C., stirring at a speed of 500 r / min for 120 min; after naturally cooling to room temperature, adding 0.8% of diethanolamine, and dispersing at high speed to fully mix to obtain a material;

[0042] (4) After drying the mixed material in step (3), the mixed material is introduced into a calcining furnace and calcined at 300° C. for 5 h in a nitrogen atmosphere. After cooling to room temperature naturally, the mixed material is ground to obtain a surface-treated iron oxide red pigment. Figure 1 shown.

[0043] Example 3

[0044] A surface treatment process for iron oxide pigments, the steps are as follows:

[0045] (1) Pour the iron oxide red pigment and deionized water into a mixer, mix and stir to prepare a 50% slurry;

[0046] (2) adding nano silicon dioxide to the slurry of step (1) at a silicon-iron ratio of 1.5:10, adding nano zirconium oxide to the slurry of step (1) at a zirconium-iron ratio of 0.2:10, and adding nano titanium dioxide to the slurry of step (1) at a titanium-iron ratio of 2.5:10, heating to 60° C., stirring at 100 r / min for 15 min, and obtaining a mixed slurry;

[0047] (3) adding 10% of epoxy resin and 6% of polyamide to the mixed slurry obtained in step (2), and then continuing to heat to 145° C., stirring at a speed of 500 r / min for 90 min; after naturally cooling to room temperature, adding 1% of isopropanolamine, dispersing at high speed to fully mix, and obtaining a material;

[0048] (4) After drying the mixed material in step (3), the mixed material is introduced into a calcining furnace and calcined at 250° C. for 8 h in a nitrogen atmosphere. After cooling naturally to room temperature, the mixed material is ground and pulverized to obtain a surface-treated iron oxide red pigment.

[0049] Example 4

[0050] A surface treatment process for iron oxide pigments, the steps are as follows:

[0051] (1) Pour the iron oxide red pigment and deionized water into a mixer, mix and stir to prepare a 55% slurry;

[0052] (2) adding nano silicon dioxide to the slurry of step (1) at a silicon-iron ratio of 1.0:10, adding nano zirconium oxide to the slurry of step (1) at a zirconium-iron ratio of 0.3:10, and adding nano titanium dioxide to the slurry of step (1) at a titanium-iron ratio of 1.5:10, heating to 60° C., stirring at 100 r / min for 15 min, and obtaining a mixed slurry;

[0053] (3) adding 25% of epoxy resin and 4% of polyamide to the mixed slurry obtained in step (2), and then continuing to heat to 145° C., stirring at a speed of 500 r / min for 50 to 120 min; after naturally cooling to room temperature, adding 0.6% of N,N-dimethylethanolamine, and dispersing at high speed to fully mix to obtain a material;

[0054] (4) After drying the mixed material in step (3), the mixed material is introduced into a calcining furnace and calcined at 280° C. for 6 h in a nitrogen atmosphere. After naturally cooling to room temperature, the mixed material is ground to obtain a surface-treated iron oxide red pigment.

[0055] Example 5

[0056] A surface treatment process for iron oxide pigments, the steps are as follows:

[0057] (1) Pour the iron oxide red pigment and deionized water into a mixer, mix and stir to prepare a 60% slurry;

[0058] (2) adding nano silicon dioxide to the slurry of step (1) at a silicon-iron ratio of 0.5:10, adding nano zirconium oxide to the slurry of step (1) at a zirconium-iron ratio of 0.4:10, and adding nano titanium dioxide to the slurry of step (1) at a titanium-iron ratio of 1:10, heating to 60° C., stirring at 100 r / min for 15 min, and obtaining a mixed slurry;

[0059] (3) adding 20% ​​of epoxy resin and 8% of polyamide to the mixed slurry obtained in step (2), and then continuing to heat to 145° C., stirring at a speed of 500 r / min for 90 min; after naturally cooling to room temperature, adding 0.8% of triethanolamine, and dispersing at high speed to fully mix to obtain a material;

[0060] (4) After drying the mixed material in step (3), the mixed material is introduced into a calcining furnace and calcined at 300° C. for 8 h in a nitrogen atmosphere. After naturally cooling to room temperature, the mixed material is ground to obtain a surface-treated iron oxide red pigment.

[0061] Example 6

[0062] A surface treatment process for iron oxide pigments, the steps are as follows:

[0063] (1) Pour the iron oxide red pigment and deionized water into a mixer, mix and stir to prepare a 65% slurry;

[0064] (2) adding nano silicon dioxide to the slurry of step (1) at a silicon-iron ratio of 0.5:10, adding nano zirconium oxide to the slurry of step (1) at a zirconium-iron ratio of 0.4:10, and adding nano titanium dioxide to the slurry of step (1) at a titanium-iron ratio of 0.5:10, heating to 60° C., stirring at 100 r / min for 15 min, and obtaining a mixed slurry;

[0065] (3) adding 20% ​​of epoxy resin and 8% of polyamide to the mixed slurry obtained in step (2), and then continuing to heat to 145° C., stirring at a speed of 500 r / min for 50 to 120 min; after naturally cooling to room temperature, adding 0.5% of isopropanolamine, and dispersing at high speed to fully mix to obtain a material;

[0066] (4) After drying the mixed material in step (3), the mixed material is introduced into a calcining furnace and calcined at 250° C. for 8 h in a nitrogen atmosphere. After naturally cooling to room temperature, the mixed material is ground to obtain a surface-treated iron oxide red pigment.

[0067] Example 7

[0068] A surface treatment process for iron oxide pigments, the steps are as follows:

[0069] (1) Pour the iron oxide red pigment and deionized water into a mixer, mix and stir to prepare a 70% slurry;

[0070] (2) adding nano silicon dioxide to the slurry of step (1) at a silicon-iron ratio of 0.1:10, adding nano zirconium oxide to the slurry of step (1) at a zirconium-iron ratio of 0.1:10, and adding nano titanium dioxide to the slurry of step (1) at a titanium-iron ratio of 1:5, heating to 60° C., stirring at 100 r / min for 15 min, and obtaining a mixed slurry;

[0071] (3) adding 5% epoxy resin and 5% polyamide to the mixed slurry obtained in step (2), and then continuing to heat to 145° C., stirring at a speed of 500 r / min for 50 to 120 min; after naturally cooling to room temperature, adding 0.7% diethanolamine, and dispersing at high speed to fully mix to obtain a material;

[0072] (4) After drying the mixed material in step (3), the mixed material is introduced into a calcining furnace and calcined at 250° C. for 6 hours under a nitrogen atmosphere. After cooling naturally to room temperature, the mixed material is ground and pulverized to obtain a surface-treated iron oxide red pigment.

[0073] Comparative Example 1

[0074] A blank control was set up, using the same iron oxide red pigment as in the example, but without any treatment on the iron oxide red pigment. Figure 2 shown.

[0075] Comparative Example 2

[0076] (1) Pour the iron oxide red pigment and deionized water into a mixer, mix and stir to prepare a 60% slurry;

[0077] (2) adding nano silicon dioxide to the slurry of step (1) at a silicon-iron ratio of 1:5, adding nano zirconium oxide to the slurry of step (1) at a zirconium-iron ratio of 1:10, and adding nano titanium dioxide to the slurry of step (1) at a titanium-iron ratio of 2:5, heating to 60° C., stirring at 100 r / min for 15 min, and obtaining a mixed slurry;

[0078] (3) adding 30% of epoxy resin and 2% of polyamide to the mixed slurry obtained in step (2), and then continuing to heat to 145° C., stirring at a speed of 500 r / min for 50 to 120 min; after naturally cooling to room temperature, adding 1% of diethanolamine, and dispersing at high speed to fully mix to obtain a material;

[0079] (4) After drying the mixed material in step (3), the mixed material is introduced into a calcining furnace and calcined at 250° C. for 8 h in a nitrogen atmosphere. After cooling naturally to room temperature, the mixed material is ground and pulverized to obtain a surface-treated iron oxide red pigment.

[0080] Comparative Example 3

[0081] A surface treatment process for iron oxide pigments, the steps are as follows:

[0082] (1) Pour the iron oxide red pigment and deionized water into a mixer, mix and stir to prepare a 60% slurry;

[0083] (2) adding nano silicon dioxide to the slurry of step (1) at a silicon-iron ratio of 1.5:10, adding nano zirconium oxide to the slurry of step (1) at a zirconium-iron ratio of 0.3:10, and adding nano titanium dioxide to the slurry of step (1) at a titanium-iron ratio of 0.5:10, heating to 60° C., stirring at 100 r / min for 15 min, and obtaining a mixed slurry;

[0084] (3) adding 2% epoxy resin and 1.5% polyamide to the mixed slurry obtained in step (2), and then continuing to heat to 145° C., stirring at a speed of 500 r / min for 50 to 120 min; after naturally cooling to room temperature, adding 0.5% diethanolamine, and dispersing at high speed to fully mix to obtain a material;

[0085] (4) After drying the mixed material in step (3), the mixed material is introduced into a calcining furnace and calcined at 300° C. for 5 h in a nitrogen atmosphere. After naturally cooling to room temperature, the mixed material is ground and pulverized to obtain a surface-treated iron oxide red pigment.

[0086] The iron oxide red pigment products obtained in the above-mentioned embodiments 2 to 7 and comparative examples 1 to 3 were tested for their color, weather resistance and wear resistance, and the test methods were as follows: the color test adopted the color comparison method, using the iron oxide red card as a reference, placing the sample to be tested in the blank space in the middle of the color card, and using a color picker to measure the color of the iron oxide red pigment, with the standard sample being 100%; the weather resistance test method was as follows: the iron oxide pigment sample was placed in an accelerated weathering instrument, and after 1000 hours of artificial climate test, the color change was observed by comparing it with the standard sample, and the numbers 1 to 8 were used to represent it, and the larger the number, the better the weather resistance; the wear resistance test method was as follows: the friction and wear performance of the sample was tested according to the ASTM G99-04 standard, and the friction coefficient and wear rate (×10 -6 mm 3 The value of (N·m) reflects the wear resistance. The test results are shown in Table 1 below.

[0087] Table 1 Performance comparison of surface treated iron oxide red pigments obtained in Examples 2 to 7 and Comparative Examples 1 to 3

[0088] color(%) Weather resistance Friction coefficient <![CDATA[Wear rate (×10 -6 mm 3 / N·m)]]> Example 2 99 8 0.65 1.29 Example 3 98 8 0.81 2.36 Example 4 96 8 0.73 2.30 Example 5 97 8 0.66 1.65 Example 6 96 7 0.68 1.75 Example 7 98 8 0.89 2.56 Comparative Example 1 100 5 3.2 8.34 Comparative Example 2 98 6 1.9 5.32 Comparative Example 3 97 7 1.3 4.21

[0089] It can be seen from the data of each embodiment and comparative example in Table 1 that the colors of embodiments 2 to 7 of the present invention are equivalent to those of comparative example 1, but the weather resistance is significantly higher than that of comparative example 1. This phenomenon is related to the fact that the present invention uses nano silicon dioxide and nano titanium dioxide to be compositely coated on the surface of the iron oxide pigment with organic sol. The nano silicon dioxide and nano titanium dioxide themselves have high ultraviolet shielding performance and weather resistance, and are coated on the surface of the iron oxide to reduce the area of ​​the iron oxide pigment exposed to the outside and in direct contact with the air, which effectively reduces the aging rate of the iron oxide pigment. The present invention adds nano silicon dioxide and nano titanium dioxide on the basis of adding nano zirconium dioxide when preparing the coating material. Since nano zirconium dioxide has ultrahigh strength and high toughness, it has excellent wear resistance after composite pigment. It can be seen from Table 1 that within the scope defined by the present invention, the higher the content of nano zirconium dioxide, the lower the friction coefficient and wear rate of the composite iron oxide pigment, and the better its wear resistance.

[0090] From the comparison of Examples 2 to 7 with Comparative Example 2, it can be seen that when preparing the coating layer material, if the amount of nanomaterial added is too much and exceeds the range specified in the present invention, most of the coated composite materials will agglomerate, making it difficult to form a coating layer, which has a great impact on the performance of the final pigment product; from the comparison of Examples 2 to 7 with Comparative Example 3, it is found that the amount of organic resin and polyamide added is small, resulting in insufficient product bonding strength. In a short period of time, the performance is not much different from that of the embodiment, but over time, the pigment is prone to fall off and the aging resistance is poor.

[0091] The present invention combines nano-silicon dioxide, nano-titanium dioxide and nano-zirconium dioxide colloidal particles with additives such as organic sols to self-assemble and coat the surface of iron oxide pigment particles layer by layer, which can effectively improve the surface state of the iron oxide pigment and greatly improve the wear resistance and aging resistance of the iron oxide pigment without affecting the gloss and color.

[0092] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A surface treatment process for improving the weather resistance of iron oxide pigments, characterized in that: Add nanomaterials to the slurry prepared with red iron oxide pigment, heat and stir to obtain a mixed slurry; then add an organic adhesive and a curing agent to the mixed slurry, stir at high temperature, add a dispersant after cooling, fully mix to obtain the material, dry, roast, cool and grind to obtain the surface-treated red iron oxide pigment.

2. The surface treatment process for improving the weather resistance of iron oxide pigment according to claim 1, characterized in that: The iron oxide red slurry is prepared by mixing and stirring the iron oxide red pigment and deionized water, and the concentration is 45-70%.

3. The surface treatment process for improving the weather resistance of iron oxide pigment according to claim 1, characterized in that: The nano materials are nano silicon dioxide, nano zirconium dioxide and nano titanium dioxide.

4. The surface treatment process for improving the weather resistance of iron oxide pigment according to claim 1, characterized in that: The proportions of added nanomaterials are: silicon: zirconium: titanium: iron 0.1~1.5:0.1~0.5:0.5~3:

10.

5. The surface treatment process for improving the weather resistance of iron oxide pigment according to claim 4, characterized in that: The ratio of added nanomaterials is: silicon: zirconium: titanium: iron is 1.5:0.5:3:

10.

6. The surface treatment process for improving the weather resistance of iron oxide pigment according to claim 1, characterized in that: The organic adhesive is epoxy resin; and the curing agent is polyamide.

7. The surface treatment process for improving the weather resistance of iron oxide pigment according to claim 1, characterized in that: The temperature of high temperature stirring is 140℃~160℃; the stirring speed is 450~550r / min.

8. The surface treatment process for improving the weather resistance of iron oxide pigment according to claim 1, characterized in that: The dispersant is an alcoholamine dispersant, selected from one or a combination of diethanolamine, triethanolamine, isopropanolamine, and N,N-dimethylethanolamine.

9. The surface treatment process for improving the weather resistance of iron oxide pigment according to claim 1, characterized in that: The proportion of the organic adhesive added in the mixed slurry is 5-25%; the proportion of the curing agent added in the mixed slurry is 2-8%.

10. The surface treatment process for improving the weather resistance of iron oxide pigment according to any one of claims 1 to 9, characterized in that: Here are the steps: (1) mixing and stirring red iron oxide pigment and deionized water to prepare a slurry of 45-70%; (2) adding nano silicon dioxide to the slurry of step (1) at a silicon-iron ratio of 0.1 to 1.5:10, adding nano zirconium oxide to the slurry of step (1) at a zirconium-iron ratio of 0.1 to 0.5:10, and adding nano titanium dioxide to the slurry of step (1) at a titanium-iron ratio of 0.5 to 3:10, heating to 60° C., stirring at 100 r / min for 15 min, and obtaining a mixed slurry; (3) adding 5-25% of epoxy resin and 2-8% of polyamide to the mixed slurry obtained in step (2), and then continuing to heat to 145° C. and stirring at a speed of 500 r / min for 50-120 min; After naturally cooling to room temperature, add 0.5-1% alcohol amine dispersant and disperse at high speed to fully mix to obtain the material; (4) After drying the mixed material in step (3), the mixed material is introduced into a calcining furnace and calcined at a temperature of 250° C. to 300° C. for 5 to 8 hours under a nitrogen atmosphere. After naturally cooling to room temperature, the mixed material is ground to obtain a surface-treated iron oxide red pigment.