Stearic acid-based high-strength hydrophobic material and preparation method thereof

Through the coating technology of stearic acid-based materials, the activity of cement-based materials is stimulated, and the problem of difficult dispersion of stearic acid in concrete and inhibiting cement hydration is solved, the high strength and hydrophobicity are improved, and the concrete is significantly improved hydrophobic properties and water resistance.

CN118995013AActive Publication Date: 2024-11-22XIAN UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410962344.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-22
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

Stearic acid is difficult to disperse in concrete as a whole hydrophobic material, inhibits cement hydration and reduces strength.

Method used

Use stearic acid, polylactic acid powder, solvent, emulsifier, deionized water, sodium carboxymethylcellulose, anti-adhesive agent, triethyl citrate, iron oxide, polyethylene glycol, chitosan, methyl silicone oil Combination materials such as , synergists, modify stearic acid through coating technology to stimulate the activity of cement-based materials, promote cement hydration, and disperse evenly in concrete to form high-strength hydrophobic materials.

Benefits of technology

It significantly improves the hydrophobicity and water-resistant and ion erosion properties of concrete, enhances the overall hydrophobic effect and strength of concrete, avoids the generation of local pores, reduces the impact of premature release of hydrophobic materials on hydration, and realizes the environmentally friendly materials Biodegradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure HDA0005063545040000011
    Figure HDA0005063545040000011
  • Figure HDA0005063545040000012
    Figure HDA0005063545040000012
Patent Text Reader

Abstract

The invention relates to the technical field of concrete hydrophobic materials, in particular to a stearic acid-based high-strength hydrophobic material and a preparation method thereof, and the stearic acid-based high-strength hydrophobic material is prepared from stearic acid, polylactic acid powder, a solvent, an emulsifier, deionized water, sodium carboxymethyl cellulose, an anti-sticking agent, triethyl citrate, iron oxide, polyethylene glycol, chitosan, methyl silicone oil and a synergist. The stearic acid-based high-strength hydrophobic material can be uniformly dispersed in the concrete to ensure that the interior of the concrete has overall hydrophobic performance, and the stearic acid-based high-strength hydrophobic material can be uniformly dispersed in the concrete to ensure that the interior of the concrete has relatively high overall hydrophobic performance, so that the hydrophobicity of the concrete can be remarkably improved; and the outermost layer of the synergist is wrapped, so that the strength of the concrete can be remarkably improved, and the prepared hydrophobic-synergistic integrated material can make great contribution to the hydrophobic property, strength, durability and service life of the cement concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of concrete hydrophobic materials, and more specifically, to a stearic acid-based high-strength hydrophobic material and a preparation method thereof. Background Art

[0002] Concrete is the foundation of modern architecture and plays an important role in the construction field, such as marine structures, bridge engineering, salt lakes, infrastructure in saline soil areas, etc. However, the physical structure of concrete itself is porous, and it has the characteristics of hydrophilicity, permeability and hygroscopicity. In actual engineering, it is easy to have durability problems caused by water erosion, resulting in serious economic losses. At present, one of the effective measures to solve this problem is to hydrophobic modification of concrete so that concrete can effectively limit water absorption and penetration.

[0003] There are two main methods for hydrophobic modification of concrete, namely surface hydrophobic coating modification and overall hydrophobic modification. Surface hydrophobic coating modification refers to spraying hydrophobic materials on the surface of formed concrete, so that external water cannot penetrate into the interior of the concrete to achieve the effect of water blocking. It is currently the most commonly used hydrophobic technology in concrete engineering in my country. However, hydrophobic coatings generally have problems such as fragile surface structure, poor wear resistance, easy peeling, susceptibility to chemical corrosion, and difficulty in covering large areas, and their subsequent maintenance also requires a lot of manpower, material and financial resources. In order to effectively overcome the problems faced by hydrophobic coatings, research on overall hydrophobic materials for concrete is of great significance. Overall hydrophobic modification refers to the addition of hydrophobic materials into the interior of concrete, which achieves an overall hydrophobic effect by changing the surface tension in the pores and cracks. Even if the surface is worn and cracks appear, its impermeability will not be affected, and it is not easy to deteriorate and does not require regular maintenance.

[0004] Stearic acid can be used as a good hydrophobic material because of its low price and excellent hydrophobicity. However, when stearic acid is mixed into concrete and used as an overall hydrophobic material, there are the following limitations: on the one hand, stearic acid has non-wetting properties, making it difficult to be evenly dispersed in concrete at room temperature, thereby causing large pores to be produced locally in the concrete. On the other hand, the direct mixing of stearic acid can inhibit the early hydration process of cement, preventing the bonding of cement particles, which is also the key to causing the mechanical properties of concrete to decline. The above-mentioned stearic acid as the deficiency of the internal mixed type overall hydrophobic material makes the application of stearic acid in actual engineering limited, and its concrete strength is difficult to reach the application standard of actual engineering. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the difficulty of dispersing stearic acid as a whole hydrophobic material after being added to concrete, inhibiting cement hydration and reducing strength, and provide a stearic acid-based high-strength hydrophobic material and a preparation method thereof.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:

[0007] A stearic acid-based high-strength hydrophobic material is prepared from stearic acid, polylactic acid powder, solvent, emulsifier, deionized water, sodium carboxymethyl cellulose, anti-adhesive agent, triethyl citrate, iron oxide, polyethylene glycol, chitosan, methyl silicone oil and synergist.

[0008] Furthermore, the mass percentages of stearic acid, polylactic acid powder, solvent, emulsifier, deionized water, sodium carboxymethyl cellulose, anti-adhesive agent, triethyl citrate, iron oxide, polyethylene glycol, chitosan, methyl silicone oil and synergist are 15% to 20%, 14% to 18%, 20% to 30%, 1% to 2%, 20% to 25%, 0.3% to 0.5%, 5% to 6%, 1% to 1.5%, 0.6% to 1%, 0.4% to 0.6%, 1% to 2.4%, 1.2% to 1.5% and 5% to 7%, respectively.

[0009] Furthermore, the stearic acid is in powder form, has a particle size of 200 mesh, a density of 0.82 g / ml, a melting point of 69-70° C., a moisture content of 0.19% wt, and is hydrophobic.

[0010] Furthermore, the solvent is any one or a combination of chloroform, acetone and ethanol.

[0011] Furthermore, the emulsifier is any one of polysorbate and polyglycerol fatty acid ester.

[0012] Furthermore, the anti-adhesive agent is any one of glyceryl monostearate and talc.

[0013] The present invention also provides a method for preparing a stearic acid-based high-strength hydrophobic material, comprising the following steps:

[0014] S1: weigh stearic acid, polylactic acid powder, solvent, emulsifier, deionized water, sodium carboxymethyl cellulose, anti-adhesive agent, triethyl citrate, iron oxide, polyethylene glycol, chitosan, methyl silicone oil, and synergist;

[0015] S2: Pour polyethylene glycol and chitosan into water, stir and mix, add triethyl citrate to the mixture, and stir magnetically to obtain a mixed emulsion A;

[0016] S3: adding an anti-adhesive agent and iron oxide to the mixed emulsion A in sequence, and performing magnetic stirring to obtain a mixed colored emulsion B;

[0017] S4: placing polylactic acid powder in a container, adding a solvent into the container containing the polylactic acid powder, and performing magnetic stirring at room temperature to obtain a polylactic acid mixed solution C;

[0018] S5: adding an emulsifier and deionized water to the polylactic acid mixed solution C, performing magnetic stirring at room temperature, and removing the solvent by rotary evaporation to obtain a polylactic acid mixed emulsion D;

[0019] S6: adding sodium carboxymethyl cellulose to the polylactic acid mixed emulsion D, continuing stirring, and then filtering to obtain a polylactic acid emulsion E;

[0020] S7: slowly pour the mixed colored emulsion B into the stirred polylactic acid emulsion E and continue stirring, and add methyl silicone oil 5 to 10 minutes before the end of stirring to obtain a colored coating crude liquid F;

[0021] S8: sieving the crude colored coating liquid F while stirring to obtain a colored coating liquid G;

[0022] S9: Pour the coating liquid D into the stearic acid in batches, and stir while supplying the coating liquid to obtain a stearic acid-based mixture H.

[0023] S10: placing the stearic acid-based mixture H into a drying oven for drying, grinding and separating, and sieving to obtain a stearic acid-based hydrophobic material I.

[0024] S11: spraying concrete synergist into stearic acid-based hydrophobic material I, drying, repeating the process 3 times, sieving, and obtaining a crude stearic acid-based high-strength hydrophobic material J.

[0025] S12: Take out the crude stearic acid-based high-strength hydrophobic material J, and sieve it to obtain the stearic acid-based high-strength hydrophobic material.

[0026] Further, in steps S9 and S10:

[0027] Place stearic acid in an environmental box, control the temperature in the environmental box to 40-50°C, and adjust the supply rate of colored coating liquid G to 15g / min / kg-25g / min / kg. After stirring in the environmental box for 1h-2h, take it out and place it in a 40°C-50°C oven to dry for 2h to obtain stearic acid-based hydrophobic material I.

[0028] Furthermore, in step S8, the crude colored coating solution F is passed through a 100-mesh sieve, in step S10, the stearic acid-based mixture H is passed through a 40-60-mesh sieve, and in step S11, the crude stearic acid-based high-strength hydrophobic material J is passed through a 30-40-mesh sieve.

[0029] In this scheme, the synergist can stimulate the activity of cement-based materials, provide more nucleation sites for hydration products, promote the hydration process of cement-based materials, and significantly improve the long-term strength of concrete. At the same time, the bridging effect between cement particles, hydration products and synergist can improve the rheological properties and early strength of cement-based materials.

[0030] Iron oxide is not only used as a pigment, but trace amounts of iron oxide can also affect the formation of cement hydration products. When iron oxide is present, more calcium ferrite hydrate (CFH) will be generated, which can fill the pores in the cement colloid to improve the density of the concrete. At the same time, it will accelerate the hydration reaction of cement, promote the formation of calcium silicate hydrate (CSH) and calcium aluminate hydrate (CAH), and improve the strength of concrete.

[0031] The carboxyl groups in the stearic acid released in the late stage of coating can react with the hydroxyl groups in the concrete to generate hydrophobic tail chains that are grafted into the concrete, making the concrete change from hydrophilic to hydrophobic. Even if the surface is worn, the newly exposed concrete can still show hydrophobicity. At the same time, stearic acid also reacts with calcium hydroxide in the concrete, promoting cement hydration by consuming calcium hydroxide.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The present invention provides a stearic acid-based high-strength hydrophobic concrete material, which has the characteristics of releasing a synergist first and then releasing a hydrophobic solid. Releasing the synergist first can achieve high dispersibility of cement-based materials, reduce the agglomeration of cement-based materials, promote the cement hydration process, and enhance the density and strength of concrete; releasing stearic acid later makes it ineffective in the early stage of concrete curing and can weaken the ester property of the surface of the hydrophobic material, so that the material has wettability and can be evenly dispersed in the concrete, which not only avoids the large pores caused by local hydrophobicity, but also enhances the overall hydrophobic effect of the concrete, and enhances the hydrophobicity and water and ion corrosion resistance of the concrete.

[0034] (2) The coating preparation in the stearic acid-based high-strength hydrophobic material of the present invention can not only change the non-wetting property of stearic acid, but also realize the controlled release of the hydrophobic material inside under the alkaline condition of concrete, so that the hydrophobic stearic acid does not play a role in the early stage of concrete curing, thereby solving the problem that the hydrophobic material inhibits the hydration of concrete. In addition, the coating material prepared by the present invention has good environmental protection, belongs to an environmentally friendly material, can be biodegraded, and reduces the pollution of waste concrete to the environment.

[0035] (3) During the material preparation process, the material is sieved through two different sieves. By controlling the mesh size of the sieve, not only can the thickness of the coating be controlled, and then the time of stearic acid release can be controlled, reducing the impact of premature release of hydrophobic materials on the early hydration of concrete, but also the overall size of the stearic acid-based high-strength hydrophobic material can be controlled to avoid the material being too large, resulting in larger pores in the concrete, affecting the hydrophobic effect and the strength of the concrete. At the same time, the stearic acid released after the early hydration is completed can fill the pores of the concrete, making the concrete denser.

[0036] (4) The addition of trace amounts of iron oxide to the coating solution can not only determine the effect of the hydrophobic material coating, but also accelerate the hydration of cement in the concrete. The hydration product, calcium ferrite hydrate (CFH), can fill the pores of the cementitious material and improve the density and strength of the concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 The electron microscope image of stearic acid used in the embodiment of the present invention;

[0038] Figure 2 This is an electron microscope image of the stearic acid-based high-strength hydrophobic material used in the embodiment of the present invention;

[0039] Figure 3 This is an electron microscope image of the stearic acid-based high-strength hydrophobic material used in the embodiment of the present invention 3 days after application;

[0040] Figure 4 This is an electron microscope image of the stearic acid-based high-strength hydrophobic material used in the embodiment of the present invention 28 days after application. DETAILED DESCRIPTION

[0041] In order to enable those skilled in the art to better understand the inventive solution, the technical solution in the embodiment of the present invention will be clearly and completely described below. Obviously, the described embodiment is only a part of the embodiment of the present invention, rather than all the embodiments. In addition, in the following description, the description of the known structures and technologies is omitted to avoid unnecessary confusion of the concepts disclosed in the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0042] The stearic acid-based high-strength hydrophobic material in the present invention has strong hydrophobic properties and can significantly improve the hydrophobicity of concrete, and the outermost layer of the synergist can significantly improve the strength of concrete, so that the prepared hydrophobic-synergistic material can make a greater contribution to the hydrophobicity, strength, durability and service life of cement concrete.

[0043] The preparation of the stearic acid-based high-strength hydrophobic material provided by the present invention is prepared from stearic acid, polylactic acid powder, solvent, emulsifier, deionized water, sodium carboxymethyl cellulose, anti-adhesive agent, triethyl citrate, iron oxide, polyethylene glycol, chitosan, methyl silicone oil, and synergist. Among them, the solvent is any one or a combination of chloroform, acetone, and ethanol, the emulsifier is any one of polysorbate and polyglycerol fatty acid ester, and the anti-adhesive agent is any one of glyceryl monostearate and talc.

[0044] The polylactic acid emulsion is prepared from polylactic acid powder, solvent, emulsifier, deionized water, and sodium carboxymethyl cellulose. The solvent is any one or a combination of chloroform, acetone, and ethanol, and the emulsifier is polysorbate or polyglycerol fatty acid ester. The preparation method of the polylactic acid emulsion is as follows: placing the polylactic acid powder in a container, adding the solvent into the container containing the polylactic acid powder, and magnetically stirring at room temperature to obtain a polylactic acid mixed liquid; adding an emulsifier and deionized water to the polylactic acid mixed liquid, and magnetically stirring at room temperature, and removing the solvent by rotary evaporation to obtain a polylactic acid mixed emulsion; adding sodium carboxymethyl cellulose to the polylactic acid mixed emulsion, continuing to stir, and then filtering to obtain a polylactic acid emulsion.

[0045] The coating liquid prepared with polylactic acid emulsion as raw material can not only form a uniform coating on the surface of stearic acid to make stearic acid wettable, but also can more evenly adsorb the synergist to improve the working performance and strength of fresh concrete; the encapsulation of the synergist can improve the fluidity and workability of cement-based materials in concrete and promote the hydration of cement-based materials.

[0046] Specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical solution of this application fall within the protection scope of the present invention.

[0047] Embodiment 1:

[0048] This embodiment provides a stearic acid-based high-strength hydrophobic material, which is made of the following raw materials, by weight: 17.5% stearic acid, 16% polylactic acid powder, 25% solvent, 1.5% emulsifier, 22.5% deionized water, 0.4% sodium carboxymethyl cellulose, 5.5% glyceryl monostearate, 1.25% triethyl citrate, 0.8% iron oxide, 0.5% polyethylene glycol, 1.7% chitosan, 1.35% methyl silicone oil, and 6% synergist.

[0049] The preparation method of the stearic acid-based high-strength hydrophobic material in this embodiment is carried out according to the following steps:

[0050] S1: weigh the raw materials according to the proportion and set aside;

[0051] S2: Pour polyethylene glycol and chitosan into water, stir and mix, add triethyl citrate to the mixture, and stir magnetically to obtain a mixed emulsion A;

[0052] S3: adding an anti-adhesive agent and iron oxide to the mixed emulsion A in sequence, and performing magnetic stirring to obtain a mixed colored emulsion B;

[0053] S4: placing polylactic acid powder in a container, adding a solvent into the container containing the polylactic acid powder, and performing magnetic stirring at room temperature to obtain a polylactic acid mixed solution C;

[0054] S5: adding an emulsifier and deionized water to the polylactic acid mixed solution C, performing magnetic stirring at room temperature, and removing the solvent by rotary evaporation to obtain a polylactic acid mixed emulsion D;

[0055] S6: adding sodium carboxymethyl cellulose to the polylactic acid mixed emulsion D, continuing stirring, and then filtering to obtain a polylactic acid emulsion E;

[0056] S7: slowly pour the mixed colored emulsion B into the stirred polylactic acid emulsion E and continue stirring, and add methyl silicone oil 5 to 10 minutes before the end of stirring to obtain a colored coating crude liquid F;

[0057] S8: sieving the crude colored coating liquid F while stirring to obtain a colored coating liquid G;

[0058] S9: Pour the coating liquid D into the stearic acid in batches, and stir while supplying the coating liquid to obtain a stearic acid-based mixture H.

[0059] S10: placing the stearic acid-based mixture H into a drying oven for drying, grinding and separating, and sieving to obtain a stearic acid-based hydrophobic material I.

[0060] S11: spraying concrete synergist into stearic acid-based hydrophobic material I, drying, repeating the process 3 times, sieving, and obtaining a crude stearic acid-based high-strength hydrophobic material J.

[0061] S12: Take out the crude stearic acid-based high-strength hydrophobic material J, and sieve it to obtain the stearic acid-based high-strength hydrophobic material.

[0062] Performance test: In order to verify that the stearic acid-based high-strength hydrophobic material of this embodiment has good performance, the stearic acid-based high-strength hydrophobic material prepared in this embodiment is added to a mixing device together with cement for mixing, and the weight dosage is 0.3% of the weight of cement. The obtained concrete is subjected to performance tests, and the test tests include compression test, flexural test, water absorption test, and droplet roll-off test.

[0063] The experiment used C40 concrete as the object, the cement used was PO42.5 ordinary Portland cement, the sand used was medium sand with a fineness modulus of 2.7, and the gravel used was 5mm to 25mm continuously graded crushed stone.

[0064] The compressive strength of concrete is tested in accordance with the "Standard for Test Methods for Physical and Mechanical Properties of Concrete" (GB / T 50081-2019).

[0065] The water absorption test method is carried out in accordance with the test method for concrete water absorption specified in the "Standard for Test Methods for Physical and Mechanical Properties of Concrete" (GB / T 50081-2019).

[0066] The droplet roll-off test was performed using the droplet volume increase and decrease method.

[0067] The amount of hydrophobic material added is 0.3% of the amount of cement added. The performance test results of this embodiment are shown in Table 1.

[0068] Embodiment 2:

[0069] This embodiment provides a stearic acid-based high-strength hydrophobic material, which is made of the following raw materials, by weight: 20% stearic acid, 14% polylactic acid powder, 20% solvent, 2% emulsifier, 24% deionized water, 0.3% sodium carboxymethyl cellulose, 6% anti-adhesive agent, 1.2% triethyl citrate, 1% iron oxide, 0.4% polyethylene glycol, 0.5% chitosan, 1.4% methyl silicone oil, and 7% synergist.

[0070] The types and dosages of the raw materials in this example are the same as those in Example 1.

[0071] The preparation method of the stearic acid-based high-strength hydrophobic material in this embodiment is basically the same as that in Example 1.

[0072] The performance test process of this embodiment is basically the same as that of embodiment 1. The amount of hydrophobic material added is 0.5% of the amount of cement added. The performance test results of this embodiment are shown in Table 1.

[0073] Embodiment 3:

[0074] This embodiment provides a stearic acid-based high-strength hydrophobic material, which is made of the following raw materials, by weight: 15% stearic acid, 18% polylactic acid powder, 28.8% solvent, 2% emulsifier, 20% deionized water, 0.5% sodium carboxymethyl cellulose, 6% anti-adhesive agent, 1.5% triethyl citrate, 0.6% iron oxide, 0.4% polyethylene glycol, 1% chitosan, 1.2% methyl silicone oil, and 5% synergist.

[0075] The types and dosages of the raw materials in this example are the same as those in Example 1.

[0076] The preparation method of the stearic acid-based high-strength hydrophobic material in this embodiment is basically the same as that in Example 1.

[0077] The performance test process of this embodiment is basically the same as that of embodiment 1. The amount of hydrophobic material added is 0.7% of the amount of cement added. The performance test results of this embodiment are shown in Table 1.

[0078] Embodiment 4:

[0079] This embodiment provides a stearic acid-based high-strength hydrophobic material, which is made of the following raw materials, by weight: 17.4% stearic acid, 17% polylactic acid powder, 25% solvent, 1.7% emulsifier, 22% deionized water, 0.3% sodium carboxymethyl cellulose, 5.7% anti-adhesive agent, 1.3% triethyl citrate, 0.7% iron oxide, 0.5% polyethylene glycol, 1.2% chitosan, 1.2% methyl silicone oil, and 6% synergist.

[0080] The types and dosages of the raw materials in this example are the same as those in Example 1.

[0081] The preparation method of the stearic acid-based high-strength hydrophobic material in this embodiment is basically the same as that in Example 1.

[0082] The performance test process of this embodiment is basically the same as that of embodiment 1. The amount of hydrophobic material added is 0.5% of the amount of cement added. The performance test results of this embodiment are shown in Table 1.

[0083] In the above embodiments, the emulsifier is polysorbate or gelatin, and the effects are basically the same.

[0084] Comparative Example 1:

[0085] This comparative example provides ordinary concrete with the same mix ratio as that of Example 1, and the component contents of its raw materials are proportionally increased according to the mix ratio relationship in Example 1, so that the sum of the weight portions of the raw materials is 100%.

[0086] The dosage requirements of each component of concrete in this comparative example are the same as those in Example 1.

[0087] The performance test process of this comparative example is basically the same as that of Example 1. The performance test results of this comparative example are shown in Table 1.

[0088] Comparative Example 2:

[0089] In this comparative example, stearic acid is added to concrete, the only difference being that the stearic acid is not modified as described above in this comparative example, and the content of other raw materials is increased in the same proportion according to the ratio in Example 1, so that the sum of the weight portions of the raw materials is 100%.

[0090] The performance test process of this comparative example is basically the same as that of Example 1.

[0091] The dosage requirements of each component of concrete in this comparative example are the same as those in Example 1, and the amount of stearic acid added is 0.5% of the amount of cement added. The performance test results of this comparative example are shown in Table 1.

[0092] Table 1 Test results of hydrophobic material performance (all changes relative to the benchmark concrete)

[0093]

[0094] From Table 1 we can see that:

[0095] From the comparison of Examples 1-4, it can be seen that the stearic acid-based high-strength hydrophobic materials in Examples 1-4 can significantly improve the compressive strength of concrete, and the 28d compressive strength in the four groups of examples is more than 114.1% of the strength of the ordinary concrete in Comparative Example 1. The reduction in water absorption rate in 72h is relatively high, and the droplet roll-off rate at 5°C also shows a relatively high performance, which has a good hydrophobic effect.

[0096] From the comparison between Examples 1-4 and Comparative Examples 1 and 2, it can be seen that: relative to ordinary concrete, the stearic acid-based high-strength hydrophobic material provided in Examples 1-4, when used as the overall hydrophobic material of concrete, has a significant hydrophobic effect, and the 3d and 28d compressive strengths of the concrete are improved. Compared with Comparative Example 2, it can be found that the modification of stearic acid in this patent greatly improves the hydrophobicity and strength of stearic acid. Examples 1-4 have better performance than existing materials. While ensuring the hydrophobicity of concrete, it can also enhance its strength and improve the durability and impermeability of concrete.

[0097] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A stearic acid-based high-strength hydrophobic material, characterized in that: The invention is prepared from stearic acid, polylactic acid powder, solvent, emulsifier, deionized water, sodium carboxymethyl cellulose, anti-adhesive agent, triethyl citrate, iron oxide, polyethylene glycol, chitosan, methyl silicone oil and synergist.

2. The stearic acid-based high-strength hydrophobic material according to claim 1, characterized in that: The mass percentages of stearic acid, polylactic acid powder, solvent, emulsifier, deionized water, sodium carboxymethyl cellulose, anti-adhesive agent, triethyl citrate, iron oxide, polyethylene glycol, chitosan, methyl silicone oil and synergist are 15%-20%, 14%-18%, 20%-30%, 1%-2%, 20%-25%, 0.3%-0.5%, 5%-6%, 1%-1.5%, 0.6%-1%, 0.4%-0.6%, 1%-2.4%, 1.2%-1.5% and 5%-7%, respectively.

3. The stearic acid-based high-strength hydrophobic material according to claim 1 or 2, characterized in that: The stearic acid is in powder form, has a particle size of 200 meshes, a density of 0.82 g / ml, a melting point of 69-70° C., a moisture content of 0.19% wt, and is hydrophobic.

4. The stearic acid-based high-strength hydrophobic material according to claim 1 or 2, characterized in that: The solvent is any one or a combination of chloroform, acetone and ethanol.

5. The stearic acid-based high-strength hydrophobic material according to claim 1 or 2, characterized in that: The emulsifier is any one of polysorbate and polyglycerol fatty acid ester.

6. The stearic acid-based high-strength hydrophobic material according to claim 1 or 2, characterized in that: The anti-adhesive agent is any one of glyceryl monostearate and talc.

7. A method for preparing the stearic acid-based high-strength hydrophobic material according to claim 1, characterized in that: The following steps are involved: S1: weigh stearic acid, polylactic acid powder, solvent, emulsifier, deionized water, sodium carboxymethyl cellulose, anti-adhesive agent, triethyl citrate, iron oxide, polyethylene glycol, chitosan, methyl silicone oil, and synergist; S2: Pour polyethylene glycol and chitosan into water, stir and mix, add triethyl citrate to the mixture, and stir magnetically to obtain a mixed emulsion A; S3: adding an anti-adhesive agent and iron oxide to the mixed emulsion A in sequence, and performing magnetic stirring to obtain a mixed colored emulsion B; S4: placing polylactic acid powder in a container, adding a solvent into the container containing the polylactic acid powder, and performing magnetic stirring at room temperature to obtain a polylactic acid mixed solution C; S5: adding an emulsifier and deionized water to the polylactic acid mixed solution C, performing magnetic stirring at room temperature, and removing the solvent by rotary evaporation to obtain a polylactic acid mixed emulsion D; S6: adding sodium carboxymethyl cellulose to the polylactic acid mixed emulsion D, continuing to stir, and then filtering to obtain a polylactic acid emulsion E; S7: slowly pour the mixed colored emulsion B into the stirred polylactic acid emulsion E and continue stirring, and add methyl silicone oil 5 to 10 minutes before the end of stirring to obtain a colored coating crude liquid F; S8: sieving the crude colored coating liquid F while stirring to obtain a colored coating liquid G; S9: Pour the coating liquid D into the stearic acid in batches, and stir while supplying the coating liquid to obtain a stearic acid-based mixture H. S10: placing the stearic acid-based mixture H into a drying oven for drying, grinding and separating, and sieving to obtain a stearic acid-based hydrophobic material I. S11: spraying concrete synergist into stearic acid-based hydrophobic material I, drying, repeating the process 3 times, sieving, and obtaining a crude stearic acid-based high-strength hydrophobic material J. S12: Take out the crude stearic acid-based high-strength hydrophobic material J, and sieve it to obtain the stearic acid-based high-strength hydrophobic material.

8. The method for preparing a stearic acid-based high-strength hydrophobic material according to claim 7, characterized in that: In steps S9 and S10: Place stearic acid in an environmental box, control the temperature in the environmental box to 40-50°C, and adjust the supply rate of colored coating liquid G to 15g / min / kg-25g / min / kg. After stirring in the environmental box for 1h-2h, take it out and place it in a 40°C-50°C oven to dry for 2h to obtain stearic acid-based hydrophobic material I.

9. The method for preparing a stearic acid-based high-strength hydrophobic material according to claim 7, characterized in that: In step S8, the colored coating crude liquid F is passed through a 100-mesh sieve, in step S10, the stearic acid-based mixture H is passed through a 40-60-mesh sieve, and in step S11, the stearic acid-based high-strength hydrophobic material crude product J is passed through a 30-40-mesh sieve.

Citation Information

Patent Citations

  • Admixture for improving impermeability of concrete and preparation method thereof

    CN112979207A

  • Composite hydrophobic agent, preparation method and application thereof

    CN113354325A

  • Fatty acid concrete hydrophobic hole bolt material and preparation method thereof

    CN114656190A

  • Concrete long-period hydrophilic and hydrophobic integrated management and maintenance material and preparation method thereof

    CN116283003A

  • Core-shell type cement admixture as well as preparation method and application thereof