Modified polyurethane waterproof coating capable of being rapidly cured in water and preparation process
By adding additives such as sodium dodecylbenzenesulfonate, cyclopropylmethoxyamine and 1,4-cyclohexanedimethyldiisocyanate to water, the waterproof coating is slow curing, easy to corrode and not wear-resistant, and the waterproof coating is solved by adding additives such as sodium dodecylbenzenesulfonate, cyclopropylmethoxyamine and 1,4-cyclohexanedimethyldiisocyanate to water, the waterproof coating is slow to cure, easy to corrode and not wear-resistant. Problem, rapid curing and improved wear resistance and corrosion resistance, are suitable for harsh environments such as ships.
Patent Information
- Application Number
- CN202411193687.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing waterproof coatings cure slowly in environments with large humidity and temperature changes, resulting in a prolonged construction cycle, which is prone to corrosion and wear-resistant, and cannot meet the needs of ships in harsh environments.
Using modified polyurethane coatings that can cure quickly in water, the polyurethane dispersion system is adjusted by adding additives such as sodium dodecylbenzenesulfonate, cyclopropylmethoxyamine and 1,4-cyclohexanedimethyldiisocyanate. , promotes the reaction of water with polyurethane, accelerates curing, and improves the hardness and durability of the coating film.
It realizes rapid curing of the coating, enhances the wear resistance and corrosion resistance of the coating, and is suitable for long-term use in harsh environments.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a modified polyurethane waterproof coating that can be quickly cured in water and a preparation process thereof. Background Art
[0002] Ship maintenance and spraying are usually carried out in a relatively closed and humid environment. Such an environment with large changes in humidity and temperature may affect the curing speed of the coating. Coatings that fail to cure quickly will take longer to dry completely, which will not only extend the construction period and increase construction costs and time costs, but also the uncured coating will be easily affected by external factors such as dust and pollutants, which will affect the quality of the coating. Ships are in a harsh environment of alternating dry and wet conditions, salt spray and ultraviolet radiation all year round. The corrosion of their metals is more serious than that of land steel. Corrosion not only leads to a decrease in the mechanical properties of steel, but also causes marine accidents. Ships sail in the waves, and the hull is often eroded by particulate matter and seawater. Therefore, the development of a waterproof coating that cures quickly and has corrosion resistance and wear resistance is an urgent problem to be solved. Summary of the invention
[0003] The invention provides a modified polyurethane waterproof coating that can be quickly cured in water and a preparation process thereof, which solves the problems of slow curing, easy corrosion and poor wear resistance of the waterproof coating in the related art.
[0004] The technical scheme of the present invention is as follows: The present invention provides a modified polyurethane waterproof coating that can be quickly cured in water, comprising the following component raw materials in parts by weight: 10 to 30 parts of dimethyl diphenyl diisocyanate, 40 to 70 parts of polytetramethylene ether glycol, 2 to 10 parts of dioctyl phthalate, 8 to 10 parts of methyl tert-butyl ketone, 3 to 5 parts of tris(2,4-xylyl) phosphate, 3 to 5 parts of diethyltin diisopropionate, 9 to 11 parts of solvent, 6 to 8 parts of sodium dodecylbenzene sulfonate, and 5 to 7 parts of auxiliary agent; The auxiliary agent includes cyclopropylmethoxyamine and 1,4-cyclohexanedimethyl diisocyanate.
[0005] In the present invention, the addition of sodium dodecylbenzene sulfonate can improve the uniformity and stability of polyurethane, and by adjusting the properties of the polyurethane dispersion system, water is more likely to contact with the polyurethane reaction material, thereby helping to accelerate the curing process of polyurethane in water.
[0006] As a further technical solution, the relative molecular mass of the polytetramethylene ether glycol is 800-1000.
[0007] As a further technical solution, the solvent is one or more of water, ethyl acetate, and propylene glycol.
[0008] As a further technical solution, the solvent is a mixed solution of water and propylene glycol, and the mass ratio of water to propylene glycol is 1:9~19.
[0009] As a further technical solution, the solvent is a mixed solution of water and propylene glycol, and the mass ratio of water to propylene glycol is 1:11.5.
[0010] As a further technical solution, the mass ratio of the cyclopropylmethoxyamine to 1,4-cyclohexanedimethyl diisocyanate is 1:2-4.
[0011] As a further technical solution, the mass ratio of the cyclopropylmethoxyamine to 1,4-cyclohexanedimethyl diisocyanate is 1:3.
[0012] As a further technical solution, the preparation process of the modified polyurethane waterproof coating that can be quickly cured in water comprises the following steps: S1. Dehydrating dimethylbiphenyl diisocyanate, polytetramethylene ether glycol, methyl tert-butyl ketone, tri(2,4-xylyl) phosphate, and diethyltin diisopropionate; S2. Add dioctyl phthalate, solvent, sodium dodecylbenzene sulfonate and additives, stir and disperse evenly to obtain a modified polyurethane waterproof coating.
[0013] As a further technical solution, the dehydration in step S1 is vacuum drying dehydration.
[0014] As a further technical solution, the vacuum drying pressure is -0.09MPa~-0.1MPa.
[0015] As a further technical solution, the dehydration temperature in step S1 is 100°C to 130°C.
[0016] As a further technical solution, the dehydration time in step S1 is 2h~3h.
[0017] As a further technical solution, the stirring time in step S2 is 1 h to 2 h.
[0018] The working principle and beneficial effects of the present invention are: In the present invention, auxiliary agents cyclopropylmethoxyamine and 1,4-cyclohexanedimethyl diisocyanate are added. The auxiliary agents contain active amino functional groups, which can react with the isocyanate groups in the polyurethane resin and participate in the curing process of the coating, thereby enhancing the hardness and durability of the coating film, improving the adhesion between the coating and the substrate, and improving the wear resistance and weather resistance of the coating. Through cross-linking, cyclopropylmethoxyamine can also enhance the chemical corrosion resistance of the polyurethane coating, making it more suitable for waterproof coating requirements in harsh environments. 1,4-cyclohexanedimethyl diisocyanate has a high reactivity, which allows them to quickly react with polyols in the preparation of polyurethane to form high molecular polymers, thereby giving the final product good mechanical properties and durability, improving the hardness and wear resistance of the polyurethane waterproof coating, and making it more suitable for long-term use in external environments. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] In the following examples and comparative examples: Polytetramethylene ether glycol: model is PTHF 1000, manufacturer is Guangzhou Innova Chemical Co., Ltd.
[0021] Example 1 A preparation process of a modified polyurethane waterproof coating that can be quickly cured in water comprises the following steps: S1. Put 10 parts of dimethyl diphenyl diisocyanate, 40 parts of polytetramethylene ether glycol, 8 parts of methyl tert-butyl ketone, 3 parts of tris(2,4-xylyl) phosphate, and 3 parts of diethyltin diisopropionate into a vacuum drying oven, set the vacuum condition to -0.09 MPa, the dehydration temperature to 100°C, and dehydrate for 2 hours; S2. After the temperature drops to room temperature, add 2 parts of dioctyl phthalate, 9 parts of solvent (0.3 parts of water, 8.7 parts of propylene glycol), 6 parts of sodium dodecylbenzene sulfonate, and 5 parts of additives (2.5 parts of cyclopropylmethoxyamine and 2.5 parts of 1,4-cyclohexanedimethyl diisocyanate), raise the temperature to 40°C, stir for 1 hour, and disperse evenly to obtain a modified polyurethane waterproof coating.
[0022] Example 2 A preparation process of a modified polyurethane waterproof coating that can be quickly cured in water comprises the following steps: S1. Put 20 parts of dimethyl diphenyl diisocyanate, 55 parts of polytetramethylene ether glycol, 9 parts of methyl tert-butyl ketone, 4 parts of tris(2,4-xylyl) phosphate, and 4 parts of diethyltin diisopropionate into a vacuum drying oven, set the vacuum condition to -0.095 MPa, the dehydration temperature to 120°C, and dehydrate for 2.5 hours; S2. After the temperature drops to room temperature, add 6 parts of dioctyl phthalate, 10 parts of solvent (0.33 parts of water, 9.67 parts of propylene glycol), 7 parts of sodium dodecylbenzene sulfonate, and 6 parts of additives (3 parts of cyclopropylmethoxyamine, 3 parts of 1,4-cyclohexanedimethyl diisocyanate), raise the temperature to 40°C, stir for 1.5 hours, and disperse evenly to obtain a modified polyurethane waterproof coating.
[0023] Example 3 A preparation process of a modified polyurethane waterproof coating that can be quickly cured in water comprises the following steps: S1. Put 30 parts of dimethyl diphenyl diisocyanate, 70 parts of polytetramethylene ether glycol, 10 parts of methyl tert-butyl ketone, 5 parts of tris(2,4-xylyl) phosphate, and 5 parts of diethyltin diisopropionate into a vacuum drying oven, set the vacuum condition to -0.1MPa, the dehydration temperature to 130°C, and dehydrate for 3h; S2. After the temperature drops to room temperature, add 10 parts of dioctyl phthalate, 11 parts of solvent (0.37 parts of water, 10.63 parts of propylene glycol), 8 parts of sodium dodecylbenzene sulfonate, and 7 parts of additives (3.5 parts of cyclopropylmethoxyamine and 3.5 parts of 1,4-cyclohexanedimethyl diisocyanate), raise the temperature to 40°C, stir for 2 hours, and disperse evenly to obtain a modified polyurethane waterproof coating.
[0024] Example 4 Compared with Example 2, the difference of Example 4 is that the auxiliary agent is 2 parts of cyclopropylmethoxyamine and 4 parts of 1,4-cyclohexanedimethyl diisocyanate.
[0025] Example 5 Compared with Example 2, the difference of Example 5 is that the auxiliary agent is 1.5 parts of cyclopropylmethoxyamine and 4.5 parts of 1,4-cyclohexanedimethyl diisocyanate.
[0026] Example 6 Compared with Example 2, the difference of Example 6 is that the auxiliary agent is 1.2 parts of cyclopropylmethoxyamine and 4.8 parts of 1,4-cyclohexanedimethyl diisocyanate.
[0027] Example 7 Compared with Example 2, the difference of Example 7 is that the auxiliary agent is 1 part of cyclopropylmethoxyamine and 5 parts of 1,4-cyclohexanedimethyl diisocyanate.
[0028] Example 8 Compared with Example 5, the difference in Example 8 is that the solvent is 0.5 parts of water and 9.5 parts of propylene glycol.
[0029] Example 9 Compared with Example 5, the difference in Example 9 is that the solvent is 0.8 parts of water and 9.2 parts of propylene glycol.
[0030] Example 10 Compared with Example 5, the difference of Example 10 is that the solvent is 1 part of water and 9 parts of propylene glycol.
[0031] Embodiment 11 Compared with Example 5, the difference in Example 11 is that the solvent is 1.5 parts of water and 8.5 parts of propylene glycol.
[0032] Comparative Example 1 Compared with Example 2, Comparative Example 1 is different in that no auxiliary agent is added.
[0033] Comparative Example 2 Compared with Example 2, the difference of Comparative Example 2 is that the auxiliary agent is cyclopropylmethoxyamine.
[0034] Comparative Example 3 Compared with Example 2, Comparative Example 3 is different in that the auxiliary agent is 1,4-cyclohexanedimethyl diisocyanate.
[0035] The modified polyurethane waterproof coatings that can be quickly cured in water obtained in Examples 1 to 11 and Comparative Examples 1 to 3 were tested according to the following method: 1. Surface drying time: According to the test method specified in GB / T 19250-2013 "Polyurethane Waterproof Coating", test the surface drying time of the sample.
[0036] 2. Drying time: Test the drying time of the sample according to the test method specified in GB / T 19250-2013 "Polyurethane Waterproof Coating".
[0037] 3. Salt spray resistance: According to the test method specified in GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test", test the salt spray resistance of the sample for 2000h.
[0038] 4. Abrasion resistance: Test the abrasion resistance of the sample according to the test method specified in GB / T 23988-2009 "Determination of Abrasion Resistance of Coatings - Falling Sand Method".
[0039] The test results are shown in the following table: Table 1 Performance test results of coatings prepared in Examples 1 to 11 and Comparative Examples 1 to 3
[0040] Compared with Example 2, no auxiliary agent is added to Comparative Example 1, the auxiliary agent added to Comparative Example 2 is only cyclopropylmethoxyamine, and the auxiliary agent added to Comparative Example 3 is only 1,4-cyclohexanedimethyl diisocyanate. As a result, the surface drying time and actual drying time of Comparative Examples 1 to 3 are all greater than Example 2, and the salt spray resistance and wear resistance are lower than Example 2, indicating that cyclopropylmethoxyamine and 1,4-cyclohexanedimethyl diisocyanate play a synergistic role, which can accelerate the curing time of the coating and enhance the corrosion resistance and wear resistance of the coating.
[0041] Compared with Example 2, Examples 4 to 7 add cyclopropylmethoxyamine and 1,4-cyclohexanedimethyl diisocyanate in different mass ratios. As a result, the surface drying time, actual drying time, and number of bubbles of Examples 4 to 6 are all less than those of Examples 2 and 7, and the wear resistance of Examples 4 to 6 is also better than that of Examples 2 and 7, indicating that when the mass ratio of cyclopropylmethoxyamine and 1,4-cyclohexanedimethyl diisocyanate is 1:2 to 4, and the preferred mass ratio is 1:3, the coating has the fastest curing speed and the best corrosion resistance and wear resistance.
[0042] Compared with Example 5, Examples 8 to 11 added water and propylene glycol in different mass ratios. As a result, the surface drying time, actual drying time, and number of bubbles of Examples 8 to 10 were all less than those of Examples 5 and 11, and the wear resistance of Examples 8 to 10 was also better, indicating that when the mass ratio of water to propylene glycol was 1:9 to 19, and the preferred ratio was 1:11.5, the coating had the fastest curing speed and the best wear resistance and corrosion resistance.
[0043] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A modified polyurethane waterproof coating that can be quickly cured in water, characterized in that: The invention comprises the following raw materials in parts by weight: 10-30 parts of dimethyl diphenyl diisocyanate, 40-70 parts of polytetramethylene ether glycol, 2-10 parts of dioctyl phthalate, 8-10 parts of methyl tert-butyl ketone, 3-5 parts of tri(2,4-xylyl) phosphate, 3-5 parts of diethyltin diisopropionate, 9-11 parts of solvent, 6-8 parts of sodium dodecylbenzene sulfonate and 5-7 parts of auxiliary agents, wherein the auxiliary agents comprise cyclopropylmethoxyamine and 1,4-cyclohexanedimethyl diisocyanate.
2. The modified polyurethane waterproof coating that can be quickly cured in water according to claim 1, characterized in that: The relative molecular mass of the polytetramethylene ether glycol is 800-1000.
3. The modified polyurethane waterproof coating that can be quickly cured in water according to claim 1, characterized in that: The solvent is one or more of water, ethyl acetate and propylene glycol.
4. The modified polyurethane waterproof coating that can be quickly cured in water according to claim 1, characterized in that: The mass ratio of the cyclopropylmethoxyamine to 1,4-cyclohexanedimethyl diisocyanate is 1:2-4.
5. The process for preparing a modified polyurethane waterproof coating that can be quickly cured in water according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Dehydrating dimethylbiphenyl diisocyanate, polytetramethylene ether glycol, methyl tert-butyl ketone, tri(2,4-xylyl) phosphate, and diethyltin diisopropionate; S2. Add dioctyl phthalate, solvent, sodium dodecylbenzene sulfonate and additives, stir and disperse evenly to obtain a modified polyurethane waterproof coating.
6. The process for preparing a modified polyurethane waterproof coating that can be quickly cured in water according to claim 5, characterized in that: The dehydration in step S1 is vacuum drying dehydration.
7. The process for preparing a modified polyurethane waterproof coating that can be quickly cured in water according to claim 5, characterized in that: The vacuum drying pressure is -0.09MPa~-0.1MPa.
8. The process for preparing a modified polyurethane waterproof coating that can be quickly cured in water according to claim 5, characterized in that: The dehydration temperature in step S1 is 100°C to 130°C.
9. The process for preparing a modified polyurethane waterproof coating that can be quickly cured in water according to claim 5, characterized in that: The dehydration time in step S1 is 2h~3h.
10. The process for preparing a modified polyurethane waterproof coating that can be quickly cured in water according to claim 5, characterized in that: The stirring time in step S2 is 1 h to 2 h.
Citation Information
Patent Citations
Single-component polyurea modified polyurethane waterproof coating and a preparing method thereof
CN109111834A
Spraying fast-setting type double-component polyurethane waterproof paint and preparation method thereof
CN109233607A
Polyurethane latent curing agent, one-component polyurethane waterproof coating and preparation method thereof
CN109251292A
Single-component root-resistant waterproof coating and preparation method thereof
CN110499096A
Bi-component anti-sagging polyurethane waterproof coating and preparation method thereof
CN114410210A