UV (ultraviolet) hot-melt pressure-sensitive adhesive for film labels as well as preparation method and application of UV hot-melt pressure-sensitive adhesive
By using solvent-free acrylate ultraviolet curing hot melt pressure-sensitive adhesive and tackifying resin in UV hot melt pressure-sensitive adhesive for membrane labels, the improvement of membrane labels in weather resistance and adhesion is solved. , achieves higher weather resistance and adhesive properties, suitable for harsh environments and low surface energy items.
Patent Information
- Application Number
- CN202411373123.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-22
AI Technical Summary
The existing UV hot melt pressure sensitive adhesives for membrane labels still have room for improvement in weather resistance and adhesion, and it is difficult to meet high requirements when used in harsh environments.
Solvent-free acrylate ultraviolet curing hot melt pressure-sensitive adhesive is used as the master glue, combined with tackifying resin and antioxidant, and improves bonding strength and weather resistance by controlling the degree of crosslinking and exposure. It is suitable for low-surface energy products Such as PET and HDPE.
It significantly improves the weather resistance and adhesive properties of membrane labels, enhances the adaptability to harsh environments, and meets the application needs of high-end disposable bottle labels and other applications.
Smart Images

Figure BDA0005068074530000091 
Figure BDA0005068074530000092 
Figure BDA0005068074530000093
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of C09J7 / 38, and in particular to a UV hot-melt pressure-sensitive adhesive for film labels, and a preparation method and application thereof. Background Art
[0002] Film labels are widely used in the field of packaging and labeling. Their excellent properties such as high transparency, good adhesion and weather resistance make them an indispensable material in modern industrial production. With the continuous increase in market demand, the performance requirements of film labels are also constantly increasing. In particular, labels used in some harsh environments have higher requirements for their weather resistance and adhesion. Weather resistance refers to the ability of a material to maintain its performance for a long time when exposed to environmental factors such as light, heat, and moisture. High viscosity refers to the ability of a material to maintain strong adhesion on various low-surface-energy items. Traditional pressure-sensitive adhesives for film labels have certain deficiencies in weather resistance and adhesion. As a new type of adhesive, UV hot-melt pressure-sensitive adhesives have gradually been promoted in the application of film labels because of their advantages such as environmental protection, fast curing, and high adhesion, especially in removable, washable, high-end disposable bottle labels, PET bottle labels, etc. However, the performance of UV hot-melt pressure-sensitive adhesives on the market in terms of weather resistance and adhesion still has room for improvement. A Chinese patent (publication number CN117363249A) discloses an environmentally friendly UV-curable hot-melt pressure-sensitive tape with high bonding strength and a preparation method thereof. By optimizing the formula system containing cationic photocuring material, UV-curing cationic initiator, sensitizer and tackifying resin to replace structural adhesive, the application requirements of blue film of battery cells are met. However, there is still room for improvement in weather resistance and bonding performance. Summary of the invention
[0003] In order to solve the above problems, the present invention provides a UV hot melt pressure-sensitive adhesive for film labels, which adopts a specific masterbatch, a tackifying resin and an antioxidant to make the provided UV hot melt pressure-sensitive adhesive have excellent weather resistance, mechanical strength and high bonding performance, meeting the application requirements of film labels.
[0004] On one hand, the present invention provides a UV hot melt pressure sensitive adhesive for film labels, which comprises at least the following components by weight: 70-100 parts of ultraviolet light curing hot melt pressure sensitive adhesive, 5-30 parts of tackifying resin, and 0.1-2 parts of antioxidant.
[0005] As a preferred technical solution, the raw materials for preparing the UV hot melt pressure-sensitive adhesive for film labels include at least the following components by weight: 80-90 parts of ultraviolet light-curing hot melt pressure-sensitive adhesive, 10-15 parts of tackifying resin, and 0.2-1 part of antioxidant.
[0006] As a preferred technical solution, the UV-curable hot melt pressure-sensitive adhesive is a solvent-free acrylate hot melt pressure-sensitive adhesive.
[0007] As a preferred technical solution, the viscosity of the UV-curable hot-melt pressure-sensitive adhesive at 130° C. is 50-80 Pa·s, preferably 60-75 Pa·s.
[0008] As a preferred technical solution, the glass transition temperature of the UV-curable hot-melt pressure-sensitive adhesive is -50 to -20°C, preferably -45 to -30°C.
[0009] As a preferred technical solution, the UV-curable hot melt pressure-sensitive adhesive is selected from JaourUVMelt TM 072. JaourUVMelt TM 120. JaourUVMelt TM At least one of JUVM-090. Preferably, the UV-curable hot melt pressure sensitive adhesive is UVHM-PSA@JUVM-072 or UVHM-PSA@JUVM-090.
[0010] As a preferred technical solution, the tackifying resin has a softening point of 80 to 150°C and a glass transition temperature of 35 to 90°C.
[0011] As a preferred technical solution, the tackifying resin is selected from at least one of C5 petroleum resin, hydrogenated C5 petroleum resin, C9 petroleum resin, hydrogenated C9 petroleum resin, L-series modified petroleum resin, α-methylstyrene monomer resin, natural resin, and terpene phenol resin.
[0012] Preferably, the L-based modified petroleum resin is selected from at least one of L-110, L-120, L-140, and L-150.
[0013] Preferably, the α-methylstyrene monomer resin is at least one selected from Kristalex F85, Kristalex 5140, Kristalex P290, and SYLVARES SA 140.
[0014] Preferably, the natural resin is selected from hydrogenated rosin resin (Foral 85E), hydrogenated rosin glycerol ester (T3085) or hydrogenated rosin pentaerythritol ester (TF105).
[0015] As a preferred technical solution, the tackifying resin is terpene phenol resin (FT115) or hydrogenated rosin resin (Foral 85E).
[0016] As a preferred technical solution, the antioxidant is a hindered phenol antioxidant, preferably antioxidant 1010.
[0017] The invention adopts solvent-free acrylate hot-melt pressure-sensitive adhesive as the masterbatch of UV hot-melt pressure-sensitive adhesive, especially adopts ultraviolet light-curing hot-melt pressure-sensitive adhesive with a viscosity of 50-80 Pa·s at 130° C. and a glass transition temperature of -50 to -20° C., and controls the exposure amount under subsequent different coating weights to adjust the internal cross-linking degree of the UV hot-melt pressure-sensitive adhesive, thereby improving the bonding strength of the product. Meanwhile, the invention is green, environmentally friendly, and non-irritating, thus meeting the application requirements of film labels.
[0018] Furthermore, the present invention adds 10-15 parts of tackifying resin, especially hydrogenated rosin or terpene phenol resin with a softening point of 80-150°C and a glass transition temperature of 35-90°C as a tackifying resin, which achieves good compatibility with 80-90 parts of UV-curable hot melt pressure-sensitive adhesive in the system, can improve the bonding performance and wettability of the hot melt adhesive for low surface energy items such as PET and HDPE, and improve the peel strength coated on PP synthetic film and PET film by nearly 40%.
[0019] Furthermore, based on a coating weight of 15-16gsm, by controlling the UVC exposure to ≥20mJ / cm 2 (determined by EIT UVPOWER PUCK 2), overcome the influence of the introduction of tackifying resin on the degree of crosslinking (the introduced resin will have a small absorption of UVC), ensure that the UV hot melt pressure sensitive adhesive is fully exposed and crosslinked to achieve the maximum cohesive strength.
[0020] In addition, the present invention further improves the weather resistance of the UV hot melt pressure-sensitive adhesive by introducing 0.2-1 part of antioxidant 1010.
[0021] On the other hand, the present invention provides a method for preparing UV hot melt pressure sensitive adhesive for film labels, which comprises at least the following steps: heating the UV curing hot melt pressure sensitive adhesive at 150-180°C for 20-40 minutes, adding a tackifying resin and an antioxidant, and stirring and mixing to obtain the product.
[0022] The third aspect of the present invention provides an application of UV hot-melt pressure-sensitive adhesive for film labels, which is applied to washable labels, removable labels, and high-end disposable bottle labels on the surface of PP, BOPP, POF, PET, PETG, and PVC substrates.
[0023] Beneficial Effects
[0024] 1. The present invention provides a UV hot melt pressure-sensitive adhesive for film labels. A specific masterbatch is used in combination with a tackifying resin and an antioxidant, so that the provided UV hot melt pressure-sensitive adhesive has excellent weather resistance, mechanical strength and high bonding performance, meeting the application requirements of film labels.
[0025] 2. The present invention adopts solvent-free acrylate hot-melt pressure-sensitive adhesive as the masterbatch of UV hot-melt pressure-sensitive adhesive, especially adopts ultraviolet light-curing hot-melt pressure-sensitive adhesive with a viscosity of 50-80 Pa·s at 130°C and a glass transition temperature of -50 to -20°C, and controls the exposure amount under subsequent different coating weights to adjust the internal cross-linking degree of the UV hot-melt pressure-sensitive adhesive, thereby improving the bonding strength of the product. At the same time, it is green, environmentally friendly, and non-irritating, meeting the application requirements of film labels.
[0026] 3. In the present invention, 10-15 parts of tackifying resin are added, especially hydrogenated rosin or terpene phenol resin with a softening point of 80-150°C and a glass transition temperature of 35-90°C as a tackifying resin, which achieves good compatibility with 80-90 parts of UV-curable hot melt pressure-sensitive adhesive in the system, can improve the bonding performance and wettability of the hot melt adhesive for low surface energy items such as PET and HDPE, and the peel strength coated on PP synthetic film and PET film is increased by nearly 40%.
[0027] 4. The UV hot melt pressure sensitive adhesive provided by the present invention is based on a coating amount of 15-16gsm, by controlling the UVC exposure amount ≥ 20mJ / cm 2 , overcome the influence of the introduction of tackifying resin on the degree of cross-linking, ensure that the UV hot melt pressure-sensitive adhesive is fully exposed and cross-linked to achieve maximum cohesive strength.
[0028] 5. The present invention further improves the weather resistance of the UV hot melt pressure-sensitive adhesive by introducing 0.2-1 part of antioxidant 1010. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the appearance of the products provided in Examples 1-9 of the present invention after mixing, and the figures correspond to Examples 1-9 from right to left.
[0030] Figure 2 The appearance of the film obtained after exposure of the products provided in Examples 10-14 of the present invention, and the figures correspond to Examples 10-14 from right to left. DETAILED DESCRIPTION
[0031] Example 1
[0032] Embodiment 1 of the present invention provides a UV hot melt pressure-sensitive adhesive for film labels, which comprises the following components in parts by weight: 84.8 parts of ultraviolet light curing hot melt pressure-sensitive adhesive, 15 parts of tackifying resin, and 0.2 parts of antioxidant.
[0033] The UV-curable hot-melt pressure-sensitive adhesive has a viscosity of 60.60 Pa·s at 130° C., a glass transition temperature of −39° C., a model of JaourUVMelt TM 072, and is sourced from Jaour.
[0034] The tackifying resin is terpene phenol resin (FT115), which is sourced from Dongguan Fantai New Materials Co., Ltd.
[0035] The antioxidant is antioxidant 1010.
[0036] On the other hand, Example 1 of the present invention provides a method for preparing a UV hot melt pressure-sensitive adhesive for film labels, comprising the following steps: heating the UV-curable hot melt pressure-sensitive adhesive at 160° C. for 30 minutes, adding a tackifying resin and an antioxidant, and stirring and mixing for 30 minutes to obtain the adhesive.
[0037] Example 2
[0038] Embodiment 2 of the present invention provides a UV hot melt pressure-sensitive adhesive for film labels, which comprises the following components in parts by weight: 85 parts of ultraviolet light-curing hot melt pressure-sensitive adhesive and 15 parts of tackifying resin.
[0039] The UV-curable hot-melt pressure-sensitive adhesive has a viscosity of 60.60 Pa·s at 130° C., a glass transition temperature of −39° C., a model of JaourUVMelt TM 072, and is sourced from Jaour.
[0040] The tackifying resin is terpene phenol resin (FT115), which is sourced from Dongguan Fantai New Materials Co., Ltd.
[0041] On the other hand, Example 2 of the present invention provides a method for preparing a UV hot melt pressure-sensitive adhesive for film labels, comprising the following steps: heating the UV-curable hot melt pressure-sensitive adhesive at 160° C. for 30 minutes, adding a tackifying resin, and stirring and mixing for 30 minutes to obtain the adhesive.
[0042] Example 3
[0043] Embodiment 3 of the present invention provides a UV hot melt pressure-sensitive adhesive for film labels, which comprises the following components in parts by weight: 85 parts of ultraviolet light-curing hot melt pressure-sensitive adhesive and 15 parts of tackifying resin.
[0044] The UV-curable hot-melt pressure-sensitive adhesive has a viscosity of 60.60 Pa·s at 130° C., a glass transition temperature of −39° C., a model of JaourUVMelt TM 072, and is sourced from Jaour.
[0045] The tackifying resin is α-methylstyrene monomer resin SYLVARES SA 140, which is derived from Kraton.
[0046] On the other hand, Example 3 of the present invention provides a method for preparing UV hot melt pressure-sensitive adhesive for film labels, comprising the following steps: heating the UV-curing hot melt pressure-sensitive adhesive at 160°C for 30 minutes, adding a tackifying resin, and stirring and mixing for 15 minutes to produce a milky white state, indicating that the resin and the masterbatch are incompatible and phase separation occurs, so the subsequent peel force test is not performed.
[0047] Example 4
[0048] Embodiment 4 of the present invention provides a UV hot melt pressure-sensitive adhesive for film labels, which comprises the following components in parts by weight: 85 parts of ultraviolet light-curing hot melt pressure-sensitive adhesive and 15 parts of tackifying resin.
[0049] The UV-curable hot-melt pressure-sensitive adhesive has a viscosity of 60.60 Pa·s at 130° C. and a glass transition temperature of -39° C. The model is JaourUVMelt TM 072, from Jiahao.
[0050] The tackifying resin is α-methylstyrene monomer resin Kristalex P290, which is sourced from Eastman.
[0051] On the other hand, Example 4 of the present invention provides a method for preparing UV hot melt pressure-sensitive adhesive for film labels, comprising the following steps: heating the UV-curing hot melt pressure-sensitive adhesive at 160°C for 30 minutes, adding a tackifying resin, and stirring and mixing for 15 minutes to produce a milky white state, indicating that the resin is incompatible with the masterbatch, and no subsequent peel force test is performed.
[0052] Example 5
[0053] Embodiment 5 of the present invention provides a UV hot melt pressure-sensitive adhesive for film labels, which comprises the following components in parts by weight: 85 parts of ultraviolet light-curing hot melt pressure-sensitive adhesive and 15 parts of tackifying resin.
[0054] The UV-curable hot-melt pressure-sensitive adhesive has a viscosity of 60.60 Pa·s at 130° C. and a glass transition temperature of -39° C. The model is JaourUVMelt TM 072, from Jiahao.
[0055] The tackifying resin is α-methylstyrene monomer resin Kristalex 5140, which is sourced from Eastman.
[0056] On the other hand, Example 5 of the present invention provides a method for preparing UV hot melt pressure-sensitive adhesive for film labels, comprising the following steps: heating the UV-curing hot melt pressure-sensitive adhesive at 160°C for 30 minutes, adding a tackifying resin, and stirring and mixing for 15 minutes until a milky white state appears, indicating that the resin is incompatible with the masterbatch, and no subsequent peel force test is performed.
[0057] Example 6
[0058] Embodiment 6 of the present invention provides, on the one hand, a UV hot melt pressure-sensitive adhesive for film labels, which comprises the following components in parts by weight: 85 parts of ultraviolet light-curing hot melt pressure-sensitive adhesive and 15 parts of tackifying resin.
[0059] The UV-curable hot-melt pressure-sensitive adhesive has a viscosity of 60.60 Pa·s at 130° C. and a glass transition temperature of -39° C. The model is JaourUVMelt TM 072, from Jiahao.
[0060] The tackifying resin is hydrogenated rosin resin Foral 85E, which is sourced from Eastman.
[0061] On the other hand, Example 6 of the present invention provides a method for preparing UV hot melt pressure-sensitive adhesive for film labels, comprising the following steps: heating the UV-curing hot melt pressure-sensitive adhesive at 160°C for 30 minutes, adding a tackifying resin, and stirring and mixing for 15 minutes to produce a milky white state, indicating that the resin and the masterbatch are incompatible and phase separation occurs, so the subsequent peel force test is not performed.
[0062] Example 7
[0063] Embodiment 7 of the present invention provides a UV hot melt pressure-sensitive adhesive for film labels, which comprises the following components in parts by weight: 85 parts of ultraviolet light-curing hot melt pressure-sensitive adhesive and 15 parts of tackifying resin.
[0064] The UV-curable hot-melt pressure-sensitive adhesive has a viscosity of 60.60 Pa·s at 130° C. and a glass transition temperature of -39° C. The model is JaourUVMelt TM 072, from Jiahao.
[0065] The tackifying resin is α-methylstyrene monomer resin Kristalex F85, which is sourced from Eastman.
[0066] On the other hand, Example 7 of the present invention provides a method for preparing UV hot melt pressure-sensitive adhesive for film labels, comprising the following steps: heating the UV-curing hot melt pressure-sensitive adhesive at 160°C for 30 minutes, adding a tackifying resin, and stirring and mixing for 15 minutes to produce a milky white state, indicating that the resin and the masterbatch are incompatible and phase separation occurs, so the subsequent peel force test is not performed.
[0067] Example 9
[0068] Example 9 of the present invention is 100 parts of a UV-curable hot melt pressure-sensitive adhesive, the UV-curable hot melt pressure-sensitive adhesive has a viscosity of 60.60 Pa·s at 130° C., a glass transition temperature of −39° C., and a model number of JaourUVMelt TM 072, from Jiahao.
[0069] Example 10
[0070] Embodiment 10 of the present invention provides a UV hot melt pressure-sensitive adhesive for film labels, which comprises the following components in parts by weight: 90 parts of ultraviolet light-curing hot melt pressure-sensitive adhesive and 10 parts of tackifying resin.
[0071] The UV-curable hot-melt pressure-sensitive adhesive has a viscosity of 71.30 Pa·s at 130° C. and a glass transition temperature of -39° C. The model is JaourUVMelt TM 090, from Jiahao.
[0072] The tackifying resin is L-150, a modified petroleum resin from Qilong Chemical.
[0073] On the other hand, embodiment 10 of the present invention provides a method for preparing a UV hot melt pressure-sensitive adhesive for film labels, comprising the following steps: heating the UV-curable hot melt pressure-sensitive adhesive at 160° C. for 30 minutes, adding a tackifying resin, and stirring and mixing for 30 minutes to obtain the adhesive.
[0074] Embodiment 11
[0075] Embodiment 11 of the present invention provides a UV hot melt pressure-sensitive adhesive for film labels, which comprises the following components in parts by weight: 90 parts of ultraviolet light-curing hot melt pressure-sensitive adhesive and 10 parts of tackifying resin.
[0076] The UV-curable hot-melt pressure-sensitive adhesive has a viscosity of 71.30 Pa·s at 130° C. and a glass transition temperature of -39° C. The model is JaourUVMelt TM 090, from Jiahao.
[0077] The tackifying resin is terpene phenol resin (FT115), which is sourced from Dongguan Fantai New Materials Co., Ltd.
[0078] On the other hand, Example 11 of the present invention provides a method for preparing a UV hot melt pressure-sensitive adhesive for film labels, comprising the following steps: heating the UV-curable hot melt pressure-sensitive adhesive at 160° C. for 30 minutes, adding a tackifying resin, and stirring and mixing for 30 minutes to obtain the adhesive.
[0079] Example 12
[0080] Embodiment 12 of the present invention provides a UV hot melt pressure-sensitive adhesive for film labels, which comprises the following components in parts by weight: 90 parts of ultraviolet light-curing hot melt pressure-sensitive adhesive and 10 parts of tackifying resin.
[0081] The UV-curable hot-melt pressure-sensitive adhesive has a viscosity of 71.3 Pa·s at 130° C. and a glass transition temperature of -39° C. The model is JaourUVMelt TM 090, from Jiahao.
[0082] The tackifying resin is hydrogenated rosin pentaerythritol ester (TF105), which is sourced from Dongguan Fantai New Materials Co., Ltd.
[0083] On the other hand, Example 12 of the present invention provides a method for preparing a UV hot melt pressure-sensitive adhesive for film labels, comprising the following steps: heating the UV-curable hot melt pressure-sensitive adhesive at 160° C. for 30 minutes, adding a tackifying resin, and stirring and mixing for 30 minutes to obtain the result.
[0084] Embodiment 13
[0085] Embodiment 13 of the present invention provides a UV hot melt pressure-sensitive adhesive for film labels, which comprises the following components in parts by weight: 90 parts of ultraviolet light-curing hot melt pressure-sensitive adhesive and 10 parts of tackifying resin.
[0086] The UV-curable hot-melt pressure-sensitive adhesive has a viscosity of 71.30 Pa·s at 130° C. and a glass transition temperature of -39° C. The model is JaourUVMelt TM 090, from Jiahao.
[0087] The tackifying resin is hydrogenated rosin glycerol ester (T3085), which is sourced from Dongguan Fantai New Materials Co., Ltd.
[0088] On the other hand, Example 13 of the present invention provides a method for preparing a UV hot melt pressure-sensitive adhesive for film labels, comprising the following steps: heating the UV-curable hot melt pressure-sensitive adhesive at 160° C. for 30 minutes, adding a tackifying resin, and stirring and mixing for 30 minutes.
[0089] Embodiment 14
[0090] Example 14 of the present invention is 100 parts of a UV-curable hot melt pressure-sensitive adhesive, the UV-curable hot melt pressure-sensitive adhesive has a viscosity of 71.30 Pa·s at 130° C., a glass transition temperature of −39° C., and a model number of JaourUVMelt TM 090, from Jiahao.
[0091] Performance Testing Methods
[0092] 1. The appearance of the products provided in Examples 1-9 after mixing is shown in Figure 1 .
[0093] 2. The appearance of the products provided in Examples 10-14 after mixing is recorded in Table 1. The viscosity at 160°C is recorded in Table 1. The coating amount is 15-16 gsm and the UVC exposure is 20 mJ / cm 2 The appearance of the film obtained is shown in Figure 2 .
[0094] 3. The products provided in Examples 1, 2, and 9 were coated on the surface of the PET substrate at a coating amount of 70 gsm, and the UVC exposure was controlled to be 120 mJ / cm 2 The test pieces were obtained under the conditions of 100°C and 180° peeling force was obtained according to the test method for peeling strength of adhesive tape in GBT 2792-2014. Each product was tested three times in parallel. The results are shown in Table 2. The products provided in Examples 2 and 9 were aged at 80°C for one day and the 180° peeling force was tested again. Each product was tested three times in parallel. The results are shown in Table 2.
[0095] 4. The products provided in Examples 11, 13, and 14 were coated on the surface of the PP substrate at a coating amount of 15-16 gsm, and the UVC exposure was controlled to obtain the test piece. The 180° peel force was obtained by referring to the test method for peel strength of adhesive tape in GBT 2792-2014. Each product was tested three times in parallel. The results are shown in Table 3.
[0096] Table 1
[0097]
[0098] Table 2
[0099]
[0100] Table 3
[0101]
Claims
1. A UV hot melt pressure sensitive adhesive for film labels, It is characterized in that The invention comprises at least the following components by weight: 70-100 parts of UV-curable hot-melt pressure-sensitive adhesive, 5-30 parts of tackifying resin and 0.1-2 parts of antioxidant. The UV-curable hot-melt pressure-sensitive adhesive is a solvent-free acrylate hot-melt pressure-sensitive adhesive.
2. The UV hot melt pressure sensitive adhesive for film labels according to claim 1, It is characterized in that The viscosity of the UV-curable hot-melt pressure-sensitive adhesive at 130° C. is 50-80 Pa·s.
3. The UV hot melt pressure sensitive adhesive for film labels according to claim 2, It is characterized in that The glass transition temperature of the ultraviolet light curing hot melt pressure sensitive adhesive is -50 to -20°C.
4. The UV hot melt pressure sensitive adhesive for film labels according to claim 1, It is characterized in that The tackifying resin has a softening point of 80 to 150°C and a glass transition temperature of 35 to 90°C.
5. The UV hot melt pressure sensitive adhesive for film labels according to claim 4, It is characterized in that The tackifying resin is selected from at least one of C5 petroleum resin, hydrogenated C5 petroleum resin, C9 petroleum resin, hydrogenated C9 petroleum resin, L-series modified petroleum resin, α-methylstyrene monomer resin, natural resin, and terpene phenol resin.
6. The UV hot melt pressure sensitive adhesive for film labels according to claim 5, It is characterized in that The L-based modified petroleum resin is selected from at least one of L-110, L-120, L-140 and L-150.
7. The UV hot melt pressure sensitive adhesive for film labels according to claim 5, It is characterized in that The α-methylstyrene monomer resin is selected from at least one of Kristalex F85, Kristalex 5140, Kristalex P290, and SYLVARES SA 140.
8. The UV hot melt pressure sensitive adhesive for film labels according to claim 5, It is characterized in that The natural resin is selected from hydrogenated rosin resin, hydrogenated rosin glycerol ester or hydrogenated rosin pentaerythritol ester.
9. A method for preparing the UV hot melt pressure sensitive adhesive for film labels according to any one of claims 1 to 8, It is characterized in that At least the following steps are included: The ultraviolet light curing hot melt pressure sensitive adhesive is heated at 150-180° C. for 20-40 minutes, and then a tackifying resin and an antioxidant are added thereto, and the mixture is stirred and mixed to obtain the adhesive.
10. An application of the UV hot melt pressure sensitive adhesive for film labels according to any one of claims 1 to 8, It is characterized in that Washable labels, removable labels, and high-end disposable bottle labels applied to the surfaces of PP, BOPP, POF, PET, PETG, and PVC substrates.
Citation Information
Cited By
Acrylate system hot-melt pressure-sensitive adhesive and preparation method thereof