Preparation method of high-temperature-resistant flexible graphite and high-temperature-resistant flexible graphite

By impregnating flexible graphite with modified vermiculite powder and mixing it with fibers to form an antioxidant coating, the problem of oxidation and corrosion of flexible graphite at high temperatures is solved, high temperature resistance and sealing performance are improved, and the use is extended life.

CN118995135APending Publication Date: 2024-11-22CIXI HIGH NEW COXIN SEALING MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411041338.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Flexible graphite is prone to oxidation and corrosion under high-temperature oxygen-rich conditions, resulting in a decrease in sealing performance and limiting its use range.

Method used

The flexible graphite powder and modified vermiculite powder are impregnated to form an antioxidant coating, and mixed with fibers for tableting to form a high-temperature flexible graphite, preventing oxygen from entering and improving high-temperature resistance.

Benefits of technology

It significantly improves the high temperature resistance of flexible graphite, maintains sealing performance and compression rebound performance, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972464210000081
    Figure BDA0004972464210000081
  • Figure BDA0004972464210000091
    Figure BDA0004972464210000091
Patent Text Reader

Abstract

The invention discloses a preparation method of high-temperature-resistant flexible graphite and the high-temperature-resistant flexible graphite thereof, and belongs to the technical field of sealing materials, the key point of the technical scheme is that the preparation method of the high-temperature-resistant flexible graphite comprises the following preparation steps: S1, crushing a flexible graphite plate, and then sieving with a 100-mesh sieve to obtain flexible graphite powder; s2, uniformly stirring and mixing the flexible graphite powder and the modified vermiculite powder according to the weight ratio of (4-8): 1 to obtain mixed powder, soaking the mixed powder in a soaking solution at the temperature of 70-80 DEG C for 50-70 minutes, and drying the mixed powder; s3, the mixed powder obtained in the step S2 and fibers are evenly mixed and then tableted, the high-temperature-resistant flexible graphite is obtained, the weight ratio of the mixed powder to the fibers is 10: (1-3), and the effect of improving the high-temperature resistance of the flexible graphite is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sealing materials, and in particular to a preparation method of high-temperature resistant flexible graphite and the high-temperature resistant flexible graphite. Background Art

[0002] At present, various process industrial equipment are commonly used in harsh environments such as high temperature, high pressure, and high vacuum. Leaks often occur at the seals of the equipment, especially at the flange seals. These leaks not only increase costs and energy, but also cause environmental pollution and produce odors.

[0003] Among new carbon materials, flexible graphite has been widely used due to its excellent performance. Due to its special molding process, a large number of microscopic pores are stored in the molding weight during the preparation process, which makes it have excellent compressibility, rebound and low stress relaxation rate. It is widely used in the field of sealing. Flexible graphite is widely used due to its high weather resistance, radiation resistance and good self-lubricating properties. However, flexible graphite is easily oxidized and corroded under high temperature and oxygen-rich conditions. When the temperature exceeds 450°C, the flexible graphite will silently undergo oxidation weight loss, and as the temperature increases, the oxidation weight loss becomes more obvious. The oxidation weight loss seriously damages the structure of the flexible graphite, affects the sealing performance, and greatly limits the scope of use of flexible graphite. Summary of the invention

[0004] In order to solve the problem of poor high temperature resistance of existing flexible graphite, the present invention provides a preparation method of high temperature resistant flexible graphite and high temperature resistant flexible graphite.

[0005] The first aspect of the present invention provides a method for preparing high temperature resistant flexible graphite, which adopts the following technical scheme: A method for preparing high temperature resistant flexible graphite comprises the following preparation steps: S1. The flexible graphite sheet is crushed and then sieved through a 100-mesh sieve to obtain a flexible graphite powder; S2. The flexible graphite powder and the modified vermiculite powder are mixed in a weight ratio of (4-8): 1 and stirred to obtain a mixed powder, the mixed powder is immersed in an impregnation solution at a temperature of 70-80 ° C for 50-70 minutes, and then the mixed powder is dried; S3. The mixed powder obtained in step S2 and the fiber are mixed evenly and then pressed into sheets to obtain high temperature resistant flexible graphite, wherein the weight ratio of the mixed powder to the fiber is 10:(1-3).

[0006] By adopting the above technical scheme, in the present application, the flexible graphite sheet is crushed into flexible graphite powder, and then the flexible graphite powder and the modified vermiculite powder are impregnated, so that an antioxidant coating is formed on the surface of the flexible graphite powder and the modified vermiculite powder. Then, the flexible graphite powder with the antioxidant coating, the modified vermiculite powder and the fiber are mixed and flattened, so that the antioxidant coating exists inside and on the surface of the finally obtained high-temperature resistant flexible graphite sheet, which effectively prevents the entry of oxygen and improves the high-temperature resistance of the flexible graphite sheet.

[0007] Preferably, the modified vermiculite powder is obtained by the following preparation method: S1. The vermiculite powder is dried at a temperature of 90-110 ° C for 30-50 minutes; S2. The vermiculite powder obtained in step S1 is placed in a mixer with a rotation speed of 500±10rpm, a modifier solution is added dropwise at a temperature of 75-80°C, and then stirred for 10-20 minutes to obtain modified vermiculite powder; the weight ratio of the vermiculite powder to the modifier solution is (3-6):1.

[0008] By adopting the above technical solution, after the vermiculite powder is modified, the surface tension of the powder can be effectively reduced, and the agglomeration phenomenon between the powders can be weakened, so that the vermiculite powder and the flexible graphite powder can be mixed evenly, and the high temperature resistance of the flexible graphite material can be effectively improved.

[0009] Preferably, the vermiculite powder has a particle size of 45-75 microns.

[0010] By adopting the above technical scheme, when the particle size of the vermiculite powder is selected to be 45-75 microns, the agglomeration phenomenon between the vermiculite powders can be effectively reduced, and when the vermiculite powder with a particle size of 45-75 microns is used, it can effectively fill the pores of the flexible graphite powder, so that the surface of the finally obtained high-temperature resistant flexible graphite sheet is smooth and has no through holes, and after being subjected to high temperature, the high-temperature resistant flexible graphite sheet can remain intact and has a certain degree of rigidity. When the particle size of the vermiculite powder is above 75 microns, the surface of the flexible graphite sheet obtained by mixing it with the flexible graphite is not easy to crack, but there are many through holes, which reduces the antioxidant performance of the flexible graphite sheet. When the particle size of the vermiculite powder is below 45 microns, the surface of the flexible graphite sheet is smooth and basically has no through holes, but it is easy to crack, which affects the service life of the flexible graphite sheet.

[0011] Preferably, the modifier solution is a stearic acid solution having a mass concentration of 2-5% formed by dissolving stearic acid in ethanol at 50-60°C.

[0012] By adopting the above technical scheme, when the modifier is selected as a stearic acid solution, the hydroxyl group at one end of the stearic acid can chemically react with the hydroxyl group on the surface of the vermiculite powder, and the long carbon chain hydrocarbon group at the other end has a certain steric hindrance, which can effectively weaken the agglomeration phenomenon between the powder particles and promote the dispersion stability of the system.

[0013] Preferably, the impregnation liquid comprises 8-15 parts of magnesium borate, 10-14 parts of potassium dihydrogen phosphate, 8-10 parts of phosphoric acid, 5-10 parts of ethylene glycol, and 40-50 parts of water by weight; the impregnation liquid is prepared by heating water to boiling, adding magnesium borate, potassium dihydrogen phosphate and ethylene glycol and mixing evenly, and then adding phosphoric acid and stirring evenly to obtain the impregnation liquid.

[0014] Preferably, the impregnation solution comprises, by weight, 10-13 parts of magnesium borate, 12-14 parts of potassium dihydrogen phosphate, 8-10 parts of phosphoric acid, 7-10 parts of ethylene glycol, and 40-50 parts of water.

[0015] By adopting the above technical scheme, the addition of magnesium borate and potassium dihydrogen phosphate in the impregnation solution can cause a polymerization reaction as the temperature rises, and the generated polymer covers the surface and pores of the flexible graphite in a network structure, hindering the entry of oxidizing gases, and the introduction of magnesium ions makes the antioxidant phase inside the flexible graphite material more stable, thereby improving the antioxidant performance of the flexible graphite. In addition, phosphoric acid will generate a phosphorus-oxygen cross-linked phosphorus-oxygen glass structure at high temperature, which can withstand high temperatures and has high adhesion. It can be further filled in the pores of the flexible graphite, hindering oxygen from entering the interior of the flexible graphite material, thereby improving the antioxidant performance of the flexible graphite.

[0016] The addition of ethylene glycol to the impregnation liquid can effectively improve the affinity between the impregnation liquid and the flexible graphite powder and the modified vermiculite powder, and is more conducive to the encapsulation of the flexible graphite powder and the vermiculite powder by the impregnation liquid.

[0017] Preferably, the fiber is one or both of glass fiber and sepiolite fiber.

[0018] Preferably, the weight ratio of the glass fiber to the sepiolite fiber is 1:(1-3).

[0019] By adopting the above technical solution, when the fiber adopts a combination of glass fiber and sepiolite fiber, the high temperature resistance of the flexible graphite material can be effectively improved.

[0020] Preferably, the tableting conditions in step S3 are an operating temperature of 50-60° C., an operating pressure of 15-20 MPa, and a tableting time of 5-10 min.

[0021] A second aspect of the present invention provides high temperature resistant flexible graphite obtained by the above-mentioned method for preparing high temperature resistant flexible graphite.

[0022] In summary, the present invention has the following beneficial effects: After the flexible graphite powder and the modified vermiculite powder are impregnated, an anti-oxidation coating can be formed on the surfaces of the flexible graphite powder and the modified vermiculite powder. Then, the flexible graphite powder with the anti-oxidation coating, the modified vermiculite powder and the fiber are mixed and flattened, so that the anti-oxidation coating exists inside and on the surface of the finally obtained high-temperature resistant flexible graphite sheet, which effectively prevents the entry of oxygen and improves the high-temperature resistance of the flexible graphite sheet. DETAILED DESCRIPTION

[0023] The present invention is further described in detail below with reference to the embodiments.

[0024] The raw materials used in the preparation examples, embodiments and comparative examples of this application are all commercially available.

[0025] Preparation Example 1 A method for preparing modified vermiculite powder comprises the following steps: S1. The vermiculite powder having a particle size of 45-75 microns was dried at a temperature of 90 ° C for 30 minutes; S2. 3 kg of the vermiculite powder obtained in step S1 was placed in a mixer at a speed of 500 ± 10 rpm, 1 kg of the modifier solution was dropped at a temperature of 75 ° C, and then stirred for 10 minutes to obtain a modified vermiculite powder; wherein the weight ratio of the vermiculite powder to the modifier solution was 3: 1; The modifier solution is a stearic acid solution with a mass concentration of 2% formed by dissolving stearic acid in ethanol at 50°C.

[0026] Preparation Example 2 A method for preparing modified vermiculite powder comprises the following steps: S1. The vermiculite powder having a particle size of 45-75 microns was dried at a temperature of 100 ° C for 40 minutes; S2. 4 kg of the vermiculite powder obtained in step S1 was placed in a mixer at a speed of 500 ± 10 rpm, 1 kg of the modifier solution was dropped at a temperature of 75 ° C, and then stirred for 15 minutes to obtain a modified vermiculite powder; wherein the weight ratio of the vermiculite powder to the modifier solution was 4: 1; The modifier solution is a stearic acid solution with a mass concentration of 4% formed by dissolving stearic acid in ethanol at 60°C.

[0027] Preparation Example 3 A method for preparing modified vermiculite powder comprises the following steps: S1. The vermiculite powder having a particle size of 45-75 microns was dried at a temperature of 110 ° C for 50 minutes; S2. 6 kg of the vermiculite powder obtained in step S1 was placed in a mixer at a speed of 500 ± 10 rpm, 1 kg of the modifier solution was dropped at a temperature of 80 ° C, and then stirred for 20 minutes to obtain a modified vermiculite powder; wherein the weight ratio of the vermiculite powder to the modifier solution was 6: 1; The modifier solution is a stearic acid solution with a mass concentration of 5% formed by dissolving stearic acid in ethanol at 60°C.

[0028] Preparation Example 4 A method for preparing modified vermiculite powder is different from Preparation Example 2 in that vermiculite powder with a particle size of less than 45 microns is selected in step S1, and the rest is the same as Preparation Example 2.

[0029] Preparation Example 5 A method for preparing modified vermiculite powder, which is different from Preparation Example 2 in that vermiculite powder with a particle size of 75-100 microns is selected in step S1, and the rest is the same as Preparation Example 2 Example 1 A method for preparing high temperature resistant flexible graphite comprises the following preparation steps: S1. Preparation of the impregnation solution: After 40kg of water was heated to boiling, 8kg of magnesium borate, 10kg of potassium dihydrogen phosphate and 5kg of ethylene glycol were added and mixed, and 8kg of phosphoric acid was added and stirred to obtain an impregnation solution; S2. The flexible graphite sheet was crushed and then sieved through a 100-mesh sieve to obtain a flexible graphite powder; S3. Take 4kg of flexible graphite powder and 1kg of modified vermiculite powder obtained in Preparation Example 1 (ie, the weight ratio of flexible graphite powder to modified vermiculite powder is 4:1) and stir to obtain a mixed powder, and immerse the mixed powder in an impregnation solution at a temperature of 70 ° C for 50 minutes, and then dry the mixed powder; S4. Take 4 kg of the mixed powder obtained in step S3 and 0.4 kg of sepiolite fiber (i.e., the weight ratio of the mixed powder to the sepiolite fiber is 10:1) and mix them evenly. Under the conditions of operating temperature of 50°C and operating pressure of 15 MPa, press them into sheets for 5 minutes to obtain high temperature resistant flexible graphite.

[0030] Example 2 A method for preparing high temperature resistant flexible graphite comprises the following preparation steps: S1. Preparation of the impregnation solution: After 40kg of water was heated to boiling, 8kg of magnesium borate, 10kg of potassium dihydrogen phosphate and 5kg of ethylene glycol were added and mixed, and 8kg of phosphoric acid was added and stirred to obtain an impregnation solution; S2. The flexible graphite sheet was crushed and then sieved through a 100-mesh sieve to obtain a flexible graphite powder; S3. Take 6kg of flexible graphite powder and 1kg of modified vermiculite powder obtained in Preparation Example 1 (ie, the weight ratio of flexible graphite powder to modified vermiculite powder is 6:1) and stir to obtain a mixed powder, and immerse the mixed powder in an impregnation solution at a temperature of 70 ° C for 50 minutes, and then dry the mixed powder; S4. Take 5 kg of the mixed powder obtained in step S3 and 1 kg of sepiolite fiber (i.e., the weight ratio of the mixed powder to the sepiolite fiber is 10:2) and mix them evenly. Under the conditions of operating temperature of 55°C and operating pressure of 20 MPa, press them into sheets for 5 minutes to obtain high temperature resistant flexible graphite.

[0031] Example 3 A method for preparing high temperature resistant flexible graphite comprises the following preparation steps: S1. Preparation of the impregnation solution: After 40kg of water was heated to boiling, 8kg of magnesium borate, 10kg of potassium dihydrogen phosphate and 5kg of ethylene glycol were added and mixed, and 8kg of phosphoric acid was added and stirred to obtain an impregnation solution; S2. The flexible graphite sheet was crushed and then sieved through a 100-mesh sieve to obtain a flexible graphite powder; S3. Take 6kg of flexible graphite powder and 1kg of modified vermiculite powder obtained in Preparation Example 1 (ie, the weight ratio of flexible graphite powder to modified vermiculite powder is 6:1) and stir to obtain a mixed powder, and immerse the mixed powder in an impregnation solution at a temperature of 70 ° C for 50 minutes, and then dry the mixed powder; S4. Take 5 kg of the mixed powder obtained in step S3 and 1 kg of sepiolite fiber (i.e., the weight ratio of the mixed powder to the sepiolite fiber is 10:2) and mix them evenly. Under the conditions of operating temperature of 55°C and operating pressure of 20 MPa, press them into sheets for 5 minutes to obtain high temperature resistant flexible graphite.

[0032] Example 4 A method for preparing high temperature resistant flexible graphite comprises the following preparation steps: S1. Preparation of the impregnation solution: After heating 45kg of water to boiling, 10kg of magnesium borate, 12kg of potassium dihydrogen phosphate and 7kg of ethylene glycol were added and mixed, and 8kg of phosphoric acid was added and stirred to obtain an impregnation solution; S2. The flexible graphite sheet was crushed and then sieved through a 100-mesh sieve to obtain a flexible graphite powder; S3. Take 6kg of flexible graphite powder and 1kg of modified vermiculite powder obtained in Preparation Example 1 (ie, the weight ratio of flexible graphite powder to modified vermiculite powder is 6:1) and stir to obtain a mixed powder, and immerse the mixed powder in an impregnation solution at a temperature of 70 ° C for 50 minutes, and then dry the mixed powder; S4. Take 5 kg of the mixed powder obtained in step S3 and 1 kg of sepiolite fiber (i.e., the weight ratio of the mixed powder to the sepiolite fiber is 10:2) and mix them evenly. Under the conditions of operating temperature of 55°C and operating pressure of 20 MPa, press them into sheets for 5 minutes to obtain high temperature resistant flexible graphite.

[0033] Example 5 A method for preparing high temperature resistant flexible graphite comprises the following preparation steps: S1. Preparation of the impregnation solution: After heating 45kg of water to boiling, 13kg of magnesium borate, 13kg of potassium dihydrogen phosphate and 8kg of ethylene glycol were added and mixed, and 8kg of phosphoric acid was added and stirred to obtain an impregnation solution; S2. The flexible graphite sheet was crushed and then sieved through a 100-mesh sieve to obtain a flexible graphite powder; S3. Take 6kg of flexible graphite powder and 1kg of modified vermiculite powder obtained in Preparation Example 1 (ie, the weight ratio of flexible graphite powder to modified vermiculite powder is 6:1) and stir to obtain a mixed powder, and immerse the mixed powder in an impregnation solution at a temperature of 70 ° C for 50 minutes, and then dry the mixed powder; S4. Take 5 kg of the mixed powder obtained in step S3 and 1 kg of sepiolite fiber (i.e., the weight ratio of the mixed powder to the sepiolite fiber is 10:2) and mix them evenly. Under the conditions of operating temperature of 55°C and operating pressure of 20 MPa, press them into sheets for 5 minutes to obtain high temperature resistant flexible graphite.

[0034] Example 6 A method for preparing high temperature resistant flexible graphite comprises the following preparation steps: S1. Preparation of the impregnation solution: After heating 50kg of water to boiling, 15kg of magnesium borate, 14kg of potassium dihydrogen phosphate and 10kg of ethylene glycol were added and mixed, and 10kg of phosphoric acid was added and stirred to obtain an impregnation solution; S2. The flexible graphite sheet was crushed and then sieved through a 100-mesh sieve to obtain a flexible graphite powder; S3. Take 6kg of flexible graphite powder and 1kg of modified vermiculite powder obtained in Preparation Example 1 (ie, the weight ratio of flexible graphite powder to modified vermiculite powder is 6:1) and stir to obtain a mixed powder, and immerse the mixed powder in an impregnation solution at a temperature of 70 ° C for 50 minutes, and then dry the mixed powder; S4. Take 5 kg of the mixed powder obtained in step S3 and 1 kg of sepiolite fiber (i.e., the weight ratio of the mixed powder to the sepiolite fiber is 10:2) and mix them evenly. Under the conditions of operating temperature of 55°C and operating pressure of 20 MPa, press them into sheets for 5 minutes to obtain high temperature resistant flexible graphite.

[0035] Example 7 A method for preparing high temperature resistant flexible graphite, which differs from Example 5 in that the modified vermiculite powder obtained in Preparation Example 2 is used in step S3, and the rest are the same as Example 5.

[0036] Example 8 A method for preparing high temperature resistant flexible graphite, which differs from Example 5 in that the modified vermiculite powder obtained in Preparation Example 3 is used in step S3, and the rest are the same as Example 5.

[0037] Example 9 A method for preparing high temperature resistant flexible graphite, which differs from Example 5 in that the modified vermiculite powder obtained in Preparation Example 4 is used in step S3, and the rest are the same as Example 5.

[0038] Example 10 A method for preparing high temperature resistant flexible graphite, which differs from Example 5 in that the modified vermiculite powder obtained in Preparation Example 5 is used in step S3, and the rest are the same as Example 5.

[0039] Embodiment 11 A method for preparing high temperature resistant flexible graphite, which differs from Example 5 in that an equal amount of glass fiber is used instead of sepiolite fiber in step S4, and the rest is the same as Example 5.

[0040] Example 12 A method for preparing high-temperature resistant flexible graphite, which differs from Example 5 in that a composite fiber of glass fiber and sepiolite fiber is used in step S4, wherein the weight ratio of the glass fiber to the sepiolite fiber is 1:1, and the rest are the same as Example 5.

[0041] Embodiment 13 A method for preparing high-temperature resistant flexible graphite, which differs from Example 5 in that a composite fiber of glass fiber and sepiolite fiber is used in step S4, wherein the weight ratio of the glass fiber to the sepiolite fiber is 1:2, and the rest are the same as Example 5.

[0042] Embodiment 14 A method for preparing high-temperature resistant flexible graphite, which differs from Example 5 in that a composite fiber of glass fiber and sepiolite fiber is used in step S4, wherein the weight ratio of the glass fiber to the sepiolite fiber is 1:3, and the rest are the same as Example 5.

[0043] Embodiment 15 A method for preparing high temperature resistant flexible graphite, which differs from Example 11 in that an equal amount of carbon fiber is used instead of sepiolite fiber, and the rest is the same as Example 11.

[0044] Example 16 A method for preparing high temperature resistant flexible graphite, which differs from Example 5 in that an equal amount of sodium tetraborate is used instead of magnesium borate in step S1, and the rest is the same as Example 5.

[0045] Comparative Example 1 A method for preparing high temperature resistant flexible graphite, which is different from Example 5 in that the preparation steps are different, specifically as follows: S1. Preparation of impregnation solution: After heating 45 kg of water to boiling, 13 kg of magnesium borate, 13 kg of potassium dihydrogen phosphate and 8 kg of ethylene glycol are added and mixed evenly, and then 8 kg of phosphoric acid is added and stirred evenly to obtain an impregnation solution; S2. The flexible graphite sheet was crushed and then sieved through a 100-mesh sieve to obtain a flexible graphite powder; S3. Take 6kg of flexible graphite powder and immerse it in an impregnation solution at a temperature of 70°C for 50 minutes, and then dry the flexible graphite powder; S4. Take 5 kg of the flexible graphite powder obtained in step S3, 1 kg of sepiolite fiber and 1 kg of the modified vermiculite powder obtained in Preparation Example 1, mix them evenly, and press them into tablets for 5 minutes at an operating temperature of 55°C and an operating pressure of 20 MPa to obtain high-temperature resistant flexible graphite.

[0046] Comparative Example 2 A method for preparing high temperature resistant flexible graphite, which is different from Example 5 in that the content of flexible graphite powder in step S2 is 9 kg, the content of modified vermiculite powder obtained in Preparation Example 1 is 1 kg, and the rest is the same as Example 5.

[0047] Comparative Example 3 A method for preparing high temperature resistant flexible graphite is different from that of Example 5 in that unmodified vermiculite powder is used in step S2, and the particle size of the vermiculite powder is 45-75 microns, and the rest is the same as that of Example 5.

[0048] Performance Testing The high temperature resistant flexible graphite sheets obtained in the above examples and comparative examples were tested for their anti-oxidation performance, sealing performance and resilience performance. The test results are shown in Table 1.

[0049] Among them, the anti-oxidation problem is the key to the use of graphite materials as high-temperature structural materials for longevity noodles. The anti-oxidation performance is determined by placing high-temperature resistant flexible graphite sheets into a Mabo furnace for high-temperature calcination. Under the condition of 700℃ oxidation aging for 8h, the oxidation weight loss rate of the flexible graphite sheets is measured to evaluate its anti-oxidation performance. Flexible graphite with a lower oxidation weight loss rate has better anti-oxidation performance.

[0050] The compression rate and rebound rate are measured in accordance with GB / T12622-2008 "Test method for compression rate and rebound rate of pipe flange gasket".

[0051] The sealing performance of the gasket is mainly characterized by the leakage rate, and good gasket compression rebound performance is an important guarantee for reducing the leakage rate and achieving gasket sealing. The leakage rate is tested according to Method A in the test standard GB / T12385-2008 "Test method for sealing performance of gaskets for pipe flanges".

[0052] Table 1 High temperature resistant flexible graphite sheet performance test results From the table above we can see that: The high temperature resistant graphite oxide sheet obtained in the embodiment of the present application has an oxidation weight loss rate of less than 14% at 700° C. and has excellent resilience, compression performance and sealing performance.

[0053] Compared with Example 5, when the modified vermiculite powder is not treated with the impregnation liquid, the high-temperature antioxidant performance of the high-temperature resistant flexible graphite sheet obtained in Comparative Example 1 is significantly reduced compared with Example 5, and the sealing performance and compression rebound performance of the high-temperature resistant flexible graphite sheet obtained in Comparative Example 1 are both reduced. It can be seen that in this application, after the modified vermiculite powder and the flexible graphite powder are impregnated at the same time, the high temperature resistance, sealing performance and compression rebound performance of the flexible graphite sheet can be effectively improved.

[0054] Compared with Example 5, when the weight ratio of the flexible graphite powder to the modified vermiculite powder is 9:1, the oxidation weight loss rate of the flexible graphite sheet increases, indicating that the high temperature resistance of the flexible graphite sheet is reduced. It can be explained that when the weight ratio of the flexible graphite powder to the modified vermiculite powder is within the range specified in the present application, not only the high temperature resistance of the flexible graphite sheet can be improved, but also the sealing performance and compression rebound performance of the flexible graphite sheet can be effectively guaranteed.

[0055] Compared with Example 5, when unmodified vermiculite powder is used, the oxidation weight loss rate of the high temperature resistant flexible graphite sheet obtained in Comparative Example 3 is higher than that in Example 5, and the sealing performance and compression rebound performance are both reduced. It can be seen that the addition of modified vermiculite powder can help improve the high temperature resistance, sealing performance and compression rebound performance of the flexible graphite sheet.

[0056] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing high temperature resistant flexible graphite, characterized in that: The method comprises the following preparation steps: S1. The flexible graphite sheet is crushed and then sieved through a 100-mesh sieve to obtain a flexible graphite powder; S2. The flexible graphite powder and the modified vermiculite powder are stirred and mixed in a weight ratio of (4-8): 1 to obtain a mixed powder, and the mixed powder is immersed in an impregnation liquid at a temperature of 70-80° C. for 50-70 minutes, and then the mixed powder is dried; S3. The mixed powder obtained in step S2 and the fiber are mixed evenly and then pressed into sheets to obtain high temperature resistant flexible graphite, wherein the weight ratio of the mixed powder to the fiber is 10:(1-3).

2. The method for preparing a high temperature resistant flexible graphite according to claim 1, characterized in that: The modified vermiculite powder is obtained by the following preparation method: S1. The vermiculite powder is dried at a temperature of 90-110 ° C for 30-50 minutes; S2. The vermiculite powder obtained in step S1 is placed in a mixer with a rotation speed of 500±10rpm, a modifier solution is added dropwise at a temperature of 75-80°C, and then stirred for 10-20 minutes to obtain modified vermiculite powder; the weight ratio of the vermiculite powder to the modifier solution is (3-6):

1.

3. The method for preparing a high temperature resistant flexible graphite according to claim 2, characterized in that: The particle size of the vermiculite powder is 45-75 microns.

4. The method for preparing high temperature resistant flexible graphite according to claim 2, characterized in that: The modifier solution is a stearic acid solution with a mass concentration of 2-5% formed by dissolving stearic acid in ethanol at 50-60°C.

5. The method for preparing high temperature resistant flexible graphite according to claim 1, characterized in that: The impregnation solution comprises 8-15 parts of magnesium borate, 10-14 parts of potassium dihydrogen phosphate, 8-10 parts of phosphoric acid, 5-10 parts of ethylene glycol, and 40-50 parts of water in parts by weight.

6. The method for preparing high temperature resistant flexible graphite according to claim 5, characterized in that: The impregnation solution comprises 10-13 parts of magnesium borate, 12-14 parts of potassium dihydrogen phosphate, 8-10 parts of phosphoric acid, 7-10 parts of ethylene glycol and 40-50 parts of water in parts by weight.

7. The method for preparing high temperature resistant flexible graphite according to claim 1, characterized in that: The fiber is one or both of glass fiber and sepiolite fiber.

8. The method for preparing high temperature resistant flexible graphite according to claim 5, characterized in that: The weight ratio of the glass fiber to the sepiolite fiber is 1:(1-3).

9. The method for preparing high temperature resistant flexible graphite according to claim 1, characterized in that: The tableting conditions in step S3 are: operating temperature 50-60° C., operating pressure 15-20 MPa, and tableting time 5-10 min.

10. A high temperature resistant flexible graphite obtained by the method for preparing high temperature resistant flexible graphite according to any one of claims 1 to 9.