Mesoporous composite friction material with high specific surface area and polytetrafluoroethylene-silicon dioxide three-dimensional through hierarchical porous structure and application of mesoporous composite friction material

The soft template hydrolysis-condensation process is used to prepare a mesoporous composite friction material with a high specific surface area of ​​polytetrafluoroethylene-silica three-dimensional penetration through the multi-stage pore structure, which solves the high wear rate of lubricating oil additives and weak oil storage and transportation capabilities. Problem, good dispersion and low friction wear coefficient in lubricating oil are achieved.

CN118995292APending Publication Date: 2024-11-22CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411080999.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing lubricating oil additives have problems such as high wear rate, weak oil storage and transportation capacity, and high friction coefficient. Pure PTFE poor wear resistance and creep resistance, mesoporous silica materials are prone to precipitation and have poor lipophilicity. Impact lubricating performance.

Method used

The soft template hydrolysis-condensation process is used to prepare a mesoporous composite friction material with a high specific surface area of ​​polytetrafluoroethylene-silica three-dimensional penetration through the multi-stage pore structure. The specific surface area and dispersion of the material are improved through the premonomer semi-continuous emulsion polymerization process. and reduce friction and wear coefficient.

Benefits of technology

The material's oil storage and oil transportation capacity and dispersion are significantly improved, and the friction and wear coefficient is reduced. The prepared material shows good lubricating performance and stability in the lubricating oil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995292A_ABST
    Figure CN118995292A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of organic and inorganic composite materials, and particularly discloses a high-specific-surface-area mesoporous composite friction material of a polytetrafluoroethylene-silicon dioxide three-dimensional through hierarchical pore channel structure and application of the high-specific-surface-area mesoporous composite friction material. A polytetrafluoroethylene-polyacrylonitrile composite material is used as a precursor, then a silicon source reagent is added, and a soft template hydrolysis-condensation process is utilized to prepare the composite material. According to the high-specific-surface-area mesoporous composite friction material with the polytetrafluoroethylene-silicon dioxide three-dimensional through hierarchical porous structure, the low friction coefficient of polytetrafluoroethylene, the lipophilicity of polyacrylonitrile and the high-specific-surface-area multi-porous structure of mesoporous silicon dioxide are combined; and the material has excellent low friction and wear characteristics and abundant pore structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic-inorganic composite materials, and specifically discloses a mesoporous composite friction material with a high specific surface area polytetrafluoroethylene-silicon dioxide three-dimensional penetrating multi-level pore structure and its application. Background Art

[0002] In recent years, lubricant additives are gradually being recognized and accepted by people. A large part of the market for lubricant additives is in the fields of aviation, aerospace and transportation. With the gradual research on lubricants, in order to achieve the requirements of extending the oil change period, extremely low friction coefficient and acid and alkali resistance, the research and development of lubricant additives is inevitable.

[0003] Polytetrafluoroethylene has good comprehensive properties, which enables it to resist strong acids and alkalis and also exhibits excellent low temperature resistance, high temperature resistance, excellent dielectric properties, high lubricity, low friction coefficient, etc. However, there are still deficiencies in the research on polytetrafluoroethylene as a lubricant additive. Since the discovery of ordered mesoporous silica, mesoporous silica nanoparticles (MSNS) have attracted widespread attention from scholars because of their unique mesoporous structure characteristics. Mesoporous silicon-based materials have a rich mesoporous structure and good oil absorption and storage properties. During the friction process, they release the lubricating oil stored in the pores to form an oil film, which can effectively achieve lubrication.

[0004] However, pure polytetrafluoroethylene has problems such as poor wear resistance, creep resistance and poor dispersibility. This is mainly because the surface energy of PTFE material is very low, and the dispersion effect in lubricating oil is not good, causing agglomeration. In addition, PTFE has a low specific surface area and poor oil storage and transportation capacity. The shortcomings of polytetrafluoroethylene have greatly limited its application. Mesoporous silica materials are easy to precipitate, mainly because of the small particle size and high specific gravity of mesoporous silica, so it is easy to precipitate in the lubricant, reducing the dilution of the lubricant and affecting its lubricating performance. In addition, pure mesoporous silica has poor lipophilicity and a high friction coefficient. Summary of the invention

[0005] The present invention aims to solve the problems of high wear rate, weak oil storage and transportation capacity, high friction coefficient and other problems of lubricating oil additives prepared by prior art, and provides a method for preparing polytetrafluoroethylene-polyacrylonitrile-silicon dioxide mesoporous composite friction material by using soft template hydrolysis-condensation process and using it as lubricating oil additive. The material has excellent dispersibility in lubricating oil and low friction and wear coefficient.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The mesoporous composite friction material with high specific surface area and three-dimensional through-hole multi-level pore structure of polytetrafluoroethylene-silicon dioxide is a mesoporous composite material prepared by using polytetrafluoroethylene-polyacrylonitrile as precursor and utilizing a soft template hydrolysis-condensation process.

[0008] The preparation of the high specific surface area polytetrafluoroethylene-silicon dioxide three-dimensional through-multi-level pore structure mesoporous composite friction material adopts the pre-monomer semi-continuous emulsion polymerization preparation process, which is mainly divided into two steps.

[0009] (1) A polytetrafluoroethylene-polyacrylonitrile composite material, ethanol, deionized water, buffer solution, and hexadecyltrimethylammonium bromide are mixed in a certain proportion, dispersed uniformly by ultrasonication, and a silicon source reagent and cyclohexane are added dropwise thereto in proportion. The mixture is stirred and reacted under reflux conditions to obtain a mesoporous composite material containing a pore-forming agent.

[0010] Wherein, the buffer solution is ammonia water, phosphate buffer, triethanolamine or urea.

[0011] The silicon source reagent is tetraethyl orthosilicate, ethyl orthosilicate or butyl orthosilicate.

[0012] The mass ratio of polytetrafluoroethylene-polyacrylonitrile composite material, silicon source reagent, buffer solution, ethanol, deionized water, cyclohexane and hexadecyltrimethylammonium bromide is (1-5):(5-15):(0.1-3):(30-100):(30-100):(20-100):(4-20).

[0013] The ultrasonic dispersion time is 10 min-60 min, the reflux stirring hydrolysis-condensation reaction time is 6-24 h, and the reaction temperature is 25-60°C.

[0014] (2) The mesoporous composite material containing the pore-forming agent, ammonium nitrate and ethanol are mixed, and refluxed at a temperature of 40-70° C. for 16-36 hours to remove the pore-forming agent. After centrifugal washing, a mesoporous composite friction material with a high specific surface area and a three-dimensional through-hole multi-level pore structure of polytetrafluoroethylene-silicon dioxide is obtained.

[0015] Wherein, the mass ratio of the mesoporous composite material, ammonium nitrate and ethanol is (1-5): (1-10): (350-500).

[0016] The invention also provides the use of the prepared polytetrafluoroethylene-silicon dioxide mesoporous composite friction material with a high specific surface area and a three-dimensional through-multi-level pore structure in the preparation of lubricating oil.

[0017] Beneficial effects:

[0018] (1) The present invention uses polytetrafluoroethylene-polyacrylonitrile composite material as a precursor, and obtains a polytetrafluoroethylene-silicon dioxide three-dimensional multi-level pore structure with a high specific surface area through a soft template hydrolysis-condensation process reaction. The morphology is uniform and the excellent properties of each substance are retained. The specific surface area of ​​the sample is greatly increased, and the oil storage and transportation capacity of the sample is greatly improved. The prepared polytetrafluoroethylene-silicon dioxide three-dimensional multi-level pore structure has good dispersibility in lubricating oil and a low friction and wear coefficient.

[0019] (2) The present invention provides a method for preparing a mesoporous composite friction material having a high specific surface area and a three-dimensional through-hole multi-level pore structure of polytetrafluoroethylene-silicon dioxide. The preparation process is green and environmentally friendly. In combination with the low friction coefficient of polytetrafluoroethylene, the lipophilicity of polyacrylonitrile and the high specific surface area and multi-pore structure of mesoporous silica, the product structure and particle size are controllable and can be widely used. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is the infrared spectrum of the high specific surface area polytetrafluoroethylene-silicon dioxide three-dimensional penetrating multi-level pore structure mesoporous composite friction material obtained in Example 1 and polytetrafluoroethylene and mesoporous silica.

[0021] Figure 2 This is a TEM image of the high specific surface area polytetrafluoroethylene-silicon dioxide mesoporous composite friction material having a three-dimensional through-multi-level pore structure obtained in Example 1.

[0022] Figure 3 The pore size distribution diagram of the polytetrafluoroethylene-silicon dioxide mesoporous composite friction material with a high specific surface area and a three-dimensional through-hole multi-level pore structure obtained in Example 1 and polytetrafluoroethylene and mesoporous silica.

[0023] Figure 4 The friction coefficient curve of the polytetrafluoroethylene-silicon dioxide mesoporous composite friction material with a three-dimensional through-multi-level pore structure having a high specific surface area, the polytetrafluoroethylene material and the polytetrafluoroethylene-polyacrylonitrile-silicon dioxide organic-inorganic composite lubricant additive in polyalphaolefin PAO-6 base oil obtained in Example 1, when the additive addition amount is 1wt%, at room temperature, 25HZ and 100N;

[0024] Figure 5 The three-dimensional surface morphology of the friction traces after lubrication of the mesoporous composite friction material with high specific surface area and polytetrafluoroethylene-polyacrylonitrile-silica three-dimensional through-multilevel pore structure and the organic-inorganic composite lubricant additive with polytetrafluoroethylene-polyacrylonitrile-silica obtained in Example 1 in the polyalphaolefin PAO 6 base oil at an additive addition amount of 1wt%, room temperature, 25HZ and 100N. DETAILED DESCRIPTION

[0025] The present invention will be further described with reference to the following examples, but it should be understood that these examples are only for illustration and should not be construed as limitations of the present invention.

[0026] The present invention adopts a soft template hydrolysis-condensation process to synthesize a mesoporous composite friction material with a high specific surface area and a three-dimensional through-multilevel pore structure of polytetrafluoroethylene-silicon dioxide. By adjusting the amount of raw materials added and the reaction conditions during the synthesis process, a mesoporous composite friction material with a high specific surface area and a three-dimensional through-multilevel pore structure of polytetrafluoroethylene-silicon dioxide with different particle sizes can be obtained.

[0027] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known to those skilled in the art.

[0028] Example 1

[0029] (1) Mix polytetrafluoroethylene-polyacrylonitrile composite material, ethanol, deionized water, buffer solution, and hexadecyltrimethylammonium bromide in proportion, disperse them uniformly by ultrasonication, and then drop silicon source reagent and cyclohexane into the mixture. Stir and react for 15 hours under reflux at 30°C to obtain a mesoporous composite material containing a pore-forming agent; wherein the mass ratio of polytetrafluoroethylene-polyacrylonitrile composite material, silicon source reagent tetraethyl orthosilicate, ammonia buffer solution, ethanol, deionized water, cyclohexane, and hexadecyltrimethylammonium bromide is 1:8:3:50:50:60:6.

[0030] (2) The mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol were mixed in a mass ratio of (1:1:250), refluxed at 60°C for 24 hours to remove the pore-forming agent, and centrifuged and washed to obtain a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide.

[0031] Figure 1 It is a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide, and an infrared spectrum of polytetrafluoroethylene material and mesoporous silica. From the figure, it can be seen that a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide has been successfully synthesized.

[0032] Figure 2 This is a TEM image of a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide. From the image, it can be seen that a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide has been successfully synthesized. The particle size is 200nm and has a clear mesoporous structure.

[0033] Figure 3It is a mesoporous composite friction material with a high specific surface area of ​​polytetrafluoroethylene-silicon dioxide three-dimensional through-multi-level pore structure, a pore size distribution diagram of polytetrafluoroethylene material and mesoporous silica. From the figure, it can be seen that the mesoporous composite material was successfully synthesized. The successfully synthesized mesoporous composite friction material with a high specific surface area of ​​polytetrafluoroethylene-silicon dioxide three-dimensional through-multi-level pore structure is a type IV isotherm curve with an H3 type hysteresis loop, indicating the mesoporous nature of the mesoporous composite friction material with a high specific surface area of ​​polytetrafluoroethylene-silicon dioxide three-dimensional through-multi-level pore structure. The specific surface area of ​​PTFE material is 12m 2 ·g -1 The specific surface area of ​​the high specific surface area polytetrafluoroethylene-silicon dioxide three-dimensional through-multi-level pore structure mesoporous composite friction material is 529m 2 ·g -1 The successful synthesis of a high specific surface area polytetrafluoroethylene-silicon dioxide three-dimensional through-multi-level pore structure mesoporous composite friction material has greatly increased the specific surface area of ​​the material by 46 times.

[0034] Figure 4 The friction coefficient curve of the polytetrafluoroethylene-silicon dioxide mesoporous composite friction material with a three-dimensional through-multi-level pore structure having a high specific surface area, the polytetrafluoroethylene material and the polytetrafluoroethylene-polyacrylonitrile-silicon dioxide organic-inorganic composite lubricant additive in polyalphaolefin PAO-6 base oil obtained in Example 1, when the additive addition amount is 1wt%, at room temperature, 25HZ and 100N;

[0035] Figure 5 This is a three-dimensional surface morphology of the friction marks after lubrication of the mesoporous composite friction material of polytetrafluoroethylene and high specific surface area polytetrafluoroethylene-silicon dioxide three-dimensional penetrating multi-level pore structure and polytetrafluoroethylene-polyacrylonitrile-silicon dioxide organic-inorganic composite lubricant additive in polyalphaolefin PAO 6 base oil obtained in Example 1, at an additive addition amount of 1wt%, room temperature, 25HZ and 100N.

[0036] Example 2

[0037] (1) Mix polytetrafluoroethylene-polyacrylonitrile composite material, ethanol, deionized water, buffer solution, and hexadecyltrimethylammonium bromide in proportion, disperse them uniformly by ultrasonication, and then drop silicon source reagent and cyclohexane into the mixture. Stir and react for 15 hours under reflux at 30°C to obtain a mesoporous composite material containing a pore-forming agent; wherein the mass ratio of polytetrafluoroethylene-polyacrylonitrile composite material, silicon source reagent tetraethyl orthosilicate, ammonia buffer solution, ethanol, deionized water, cyclohexane, and hexadecyltrimethylammonium bromide is 1:8:1:50:50:60:6.

[0038] (2) The mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol were mixed in a mass ratio of (1:1:250), refluxed at 60°C for 24 hours to remove the pore-forming agent, and centrifuged and washed to obtain a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide.

[0039] Example 3

[0040] (1) Mix polytetrafluoroethylene-polyacrylonitrile composite material, ethanol, deionized water, buffer solution, and hexadecyltrimethylammonium bromide in proportion, disperse them uniformly by ultrasonication, and then drop silicon source reagent and cyclohexane into the mixture. Stir and react for 15 hours under reflux at 30°C to obtain a mesoporous composite material containing a pore-forming agent; wherein the mass ratio of polytetrafluoroethylene-polyacrylonitrile composite material, silicon source reagent tetraethyl orthosilicate, ammonia buffer solution, ethanol, deionized water, cyclohexane, and hexadecyltrimethylammonium bromide is 1:8:5:50:50:60:6.

[0041] (2) The mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol were mixed in a mass ratio of (1:1:250), refluxed at 60°C for 24 hours to remove the pore-forming agent, and centrifuged and washed to obtain a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide.

[0042] Example 4

[0043] (1) Mix polytetrafluoroethylene-polyacrylonitrile composite material, ethanol, deionized water, buffer solution, and hexadecyltrimethylammonium bromide in proportion, disperse them uniformly by ultrasonication, and then drop silicon source reagent and cyclohexane into the mixture. Stir and react for 15 hours under reflux at 30°C to obtain a mesoporous composite material containing a pore-forming agent; wherein the mass ratio of polytetrafluoroethylene-polyacrylonitrile composite material, silicon source reagent tetraethyl orthosilicate, ammonia buffer solution, ethanol, deionized water, cyclohexane, and hexadecyltrimethylammonium bromide is 1:8:3:50:50:60:8.

[0044] (2) The mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol were mixed in a mass ratio of (1:1:250), refluxed at 60°C for 24 hours to remove the pore-forming agent, and centrifuged and washed to obtain a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide.

[0045] Example 5

[0046] (1) Mix polytetrafluoroethylene-polyacrylonitrile composite material, ethanol, deionized water, buffer solution, and hexadecyltrimethylammonium bromide in proportion, disperse them uniformly by ultrasonication, and then drop silicon source reagent and cyclohexane into the mixture. Stir and react for 15 hours under reflux at 30°C to obtain a mesoporous composite material containing a pore-forming agent; wherein the mass ratio of polytetrafluoroethylene-polyacrylonitrile composite material, silicon source reagent tetraethyl orthosilicate, ammonia buffer solution, ethanol, deionized water, cyclohexane, and hexadecyltrimethylammonium bromide is 1:8:3:50:50:60:10.

[0047] (2) The mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol were mixed in a mass ratio of (1:1:250), refluxed at 60°C for 24 hours to remove the pore-forming agent, and centrifuged and washed to obtain a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide.

[0048] Example 6

[0049] (1) Mix polytetrafluoroethylene-polyacrylonitrile composite material, ethanol, deionized water, buffer solution, and hexadecyltrimethylammonium bromide in proportion, disperse them uniformly by ultrasonication, and then drop silicon source reagent and cyclohexane into the mixture. Stir and react for 15 hours under reflux at 30°C to obtain a mesoporous composite material containing a pore-forming agent; wherein the mass ratio of polytetrafluoroethylene-polyacrylonitrile composite material, silicon source reagent tetraethyl orthosilicate, ammonia buffer solution, ethanol, deionized water, cyclohexane, and hexadecyltrimethylammonium bromide is 1:8:3:50:50:60:4.

[0050] (2) The mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol were mixed in a mass ratio of (1:1:250), refluxed at 60°C for 24 hours to remove the pore-forming agent, and centrifuged and washed to obtain a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide.

[0051] Example 7

[0052] (1) Mix polytetrafluoroethylene-polyacrylonitrile composite material, ethanol, deionized water, buffer solution, and hexadecyltrimethylammonium bromide in proportion, disperse them uniformly by ultrasonication, and then drop silicon source reagent and cyclohexane into them. Stir and react for 15 hours under reflux conditions at 30°C to obtain a mesoporous composite material containing a pore-forming agent; wherein the mass ratio of polytetrafluoroethylene-polyacrylonitrile composite material, silicon source reagent tetraethyl orthosilicate, triethanolamine buffer solution, ethanol, deionized water, cyclohexane, and hexadecyltrimethylammonium bromide is 1:8:3:50:50:60:6.

[0053] (2) The mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol were mixed in a mass ratio of (1:1:250), refluxed at 60°C for 24 hours to remove the pore-forming agent, and centrifuged and washed to obtain a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide.

[0054] Example 8

[0055] (1) The polytetrafluoroethylene-polyacrylonitrile composite material, ethanol, deionized water, buffer solution, and hexadecyltrimethylammonium bromide were mixed in proportion, ultrasonically dispersed evenly, and then the silicon source reagent and cyclohexane were dropped in. The reaction was stirred and refluxed at 30°C for 15 hours to obtain a mesoporous composite material containing a pore-forming agent; wherein the mass ratio of the polytetrafluoroethylene-polyacrylonitrile composite material, the silicon source reagent tetraethyl orthosilicate, the urea buffer solution, ethanol, deionized water, cyclohexane, and hexadecyltrimethylammonium bromide was 1:8:3:50:50:60:6.

[0056] (2) The mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol were mixed in a mass ratio of (1:1:250), refluxed at 60°C for 24 hours to remove the pore-forming agent, and centrifuged and washed to obtain a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide.

[0057] Example 9

[0058] (1) Mix polytetrafluoroethylene-polyacrylonitrile composite material, ethanol, deionized water, buffer solution, and hexadecyltrimethylammonium bromide in proportion, disperse them uniformly by ultrasonication, and then drop silicon source reagent and cyclohexane into the mixture. Stir and react for 15 hours under reflux at 30°C to obtain a mesoporous composite material containing a pore-forming agent; wherein the mass ratio of polytetrafluoroethylene-polyacrylonitrile composite material, silicon source reagent tetraethyl orthosilicate, ammonia buffer solution, ethanol, deionized water, cyclohexane, and hexadecyltrimethylammonium bromide is 1:8:3:50:50:60:6.

[0059] (2) The mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol were mixed in a mass ratio of (3:1:250), refluxed at 60°C for 24 hours to remove the pore-forming agent, and centrifuged and washed to obtain a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide.

[0060] Example 10

[0061] (1) Mix polytetrafluoroethylene-polyacrylonitrile composite material, ethanol, deionized water, buffer solution, and hexadecyltrimethylammonium bromide in proportion, disperse them uniformly by ultrasonication, and then drop silicon source reagent and cyclohexane into the mixture. Stir and react for 15 hours under reflux at 30°C to obtain a mesoporous composite material containing a pore-forming agent; wherein the mass ratio of polytetrafluoroethylene-polyacrylonitrile composite material, silicon source reagent tetraethyl orthosilicate, ammonia buffer solution, ethanol, deionized water, cyclohexane, and hexadecyltrimethylammonium bromide is 1:8:3:50:50:60:6.

[0062] (2) The mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol were mixed in a mass ratio of (1:1:400), refluxed at 60°C for 24 hours to remove the pore-forming agent, and centrifuged and washed to obtain a mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide.

[0063] Comparative Example 1

[0064] (1) In a reaction vessel equipped with a reflux condenser, a stirrer, a thermometer and a nitrogen inlet, add 100 mL of deionized water, add 10 mL of polytetrafluoroethylene emulsion (solid content 40%-60%) into the reaction vessel, and ultrasonically disperse for 30 minutes. Add 1.875 mL of acrylonitrile monomer and 0.001 g of initiator potassium persulfate. Heat and stir to raise the temperature to 75°C. After the temperature stabilizes, use a peristaltic pump to drop the remaining 13.125 mL of acrylonitrile and 0.007 g of initiator potassium persulfate, and react at a constant temperature. Stir continuously and introduce nitrogen during the whole process. After the reaction is completed, the reaction solution is transferred out of the reaction vessel for centrifugation, the lower precipitate is repeatedly washed with tetrahydrofuran for multiple times, and finally the lower precipitate is taken out by centrifugation to obtain a solid product, which is dried to obtain a solid product, and the solid product is crushed into powder to obtain a polytetrafluoroethylene-polyacrylonitrile composite friction material.

[0065] Comparative Example 2

[0066] Weigh 6mmol (2.1867g) of hexadecyltrimethylammonium bromide in a flask, add 200mL of deionized water, and disperse ultrasonically. Stir the reaction at 30°C for 3h. After the reaction is completed, add 10mL of ethyl orthosilicate, and 17mL of ammonia water into 300mL of deionized water and mix and drip. Stir the reaction at 30°C for 8h. After the reaction is completed, pour the solution into a hydrothermal reactor and put it into an oven. The hydrothermal conditions are 90°C and 12h. After the reaction is completed, cool the mixture, take it out, wash, filter, and dry it. Finally, bake it at 400°C in a muffle furnace for 4h to obtain mesoporous silica.

[0067] Comparative Example 3

[0068] (1) Weigh 1g of polytetrafluoroethylene-polyacrylonitrile organic material into a three-necked flask, add 50mL of ethanol and ultrasonically disperse for 30min, add 1mL of ammonia water and 50mL of deionized water into the flask, stir and drop 6mL of tetraethyl orthosilicate and 1mL of ethanol at a dropping speed of 7s / drop, and continue stirring for 15h at 30°C after the dropping is completed. Centrifuge and dry the sample at a centrifugal speed of 6000rpm for 5min to obtain a polytetrafluoroethylene-polyacrylonitrile-silica organic-inorganic composite lubricating oil additive.

[0069] Test Case

[0070] The tribological test of the present invention adopts German Optimol SRV5 to evaluate the friction and wear performance of PAO-6 base lubricant containing high specific surface area polytetrafluoroethylene-silicon dioxide three-dimensional through-multi-level pore structure mesoporous composite friction material (friction material addition amount is 1%). The experimental load is 200N, the friction rate is 25HZ, the experimental time is 30min, and it is carried out at room temperature. The friction distance is 1mm. The experimental ball used is made of AISI52100 steel, 60HRC±2, Ra 0.025μm±0.005μm, with a diameter of 10mm and a hardness of HRC59-61. The friction torque is recorded during the experiment and the friction coefficient is calculated.

[0071] Table 1 shows the performance test results of high specific surface area polytetrafluoroethylene-silica three-dimensional through-multi-level pore structure mesoporous composite friction materials, polytetrafluoroethylene-polyacrylonitrile composite materials, mesoporous silica composite materials and polytetrafluoroethylene doped mesoporous silica composite materials prepared in Examples 1 to 10 and Comparative Examples 1 to 3.

[0072] Table 1

[0073]

[0074] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A mesoporous composite friction material with a high specific surface area and a three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide, characterized in that: The composite friction material is prepared by using a polytetrafluoroethylene-polyacrylonitrile composite material as a precursor, and then adding a silicon source reagent and utilizing a soft template hydrolysis-condensation process.

2. A method for preparing a mesoporous composite friction material having a high specific surface area and a three-dimensional through-hole multi-level pore structure of polytetrafluoroethylene-silicon dioxide according to claim 1, characterized in that: The preparation method of the composite friction material comprises the following steps: (1) mixing a polytetrafluoroethylene-polyacrylonitrile composite material, a buffer solution, ethanol, deionized water, and hexadecyltrimethylammonium bromide in proportion, uniformly dispersing by ultrasonication, and then dropping a silicon source reagent and cyclohexane into the mixture; stirring the mixture under reflux conditions to obtain a mesoporous composite material containing a pore-forming agent; (2) The mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol are mixed, refluxed to remove the pore-forming agent, and centrifuged and washed to obtain a mesoporous composite friction material with a high specific surface area and a three-dimensional through-hole multi-level pore structure of polytetrafluoroethylene-silicon dioxide.

3. The method for preparing the mesoporous composite friction material with high specific surface area and three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide according to claim 2, characterized in that: Step (1) The mass ratio of the polytetrafluoroethylene-polyacrylonitrile composite material, the silicon source reagent, the buffer solution, the ethanol, the deionized water, the cyclohexane and the hexadecyltrimethylammonium bromide is 1-5: 5-15: 0.1-3: 30-100: 30-100: 20-100: 4-20.

4. The method for preparing the mesoporous composite friction material with high specific surface area and three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide according to claim 2, characterized in that: The ultrasonic dispersion time of step (1) is 10 min-60 min, the reflux stirring reaction temperature is 25-60° C., and the reaction time is 6-24 h.

5. The method for preparing the mesoporous composite friction material with high specific surface area and three-dimensional multi-level pore structure of polytetrafluoroethylene-silicon dioxide according to claim 2, characterized in that: The buffer solution in step (1) is ammonia water, phosphate buffer, triethanolamine or urea.

6. The method for preparing the high specific surface area polytetrafluoroethylene-silicon dioxide three-dimensional through-multi-level pore structure mesoporous composite friction material according to claim 2, characterized in that: The silicon source reagent in step (1) is tetraethyl orthosilicate, ethyl orthosilicate or butyl orthosilicate.

7. The method for preparing the high specific surface area polytetrafluoroethylene-silicon dioxide mesoporous composite friction material having a three-dimensional through-hole multi-level pore structure according to claim 2, characterized in that: The mass ratio of the mesoporous composite material containing a pore-forming agent, ammonium nitrate and ethanol in step (2) is 1-5:1-10:350-500.

8. The method for preparing the high specific surface area polytetrafluoroethylene-silicon dioxide three-dimensional through-multi-level pore structure mesoporous composite friction material according to claim 2, characterized in that: The reflux temperature in step (2) is 40-70° C. and the reflux time is 16-36 h.

9. An application of the mesoporous composite friction material with a high specific surface area of ​​polytetrafluoroethylene-silicon dioxide three-dimensional through-multi-level pore structure according to claim 1, characterized in that: The mesoporous composite friction material with high specific surface area and polytetrafluoroethylene-silicon dioxide three-dimensional penetrating multi-level pore structure is used as a lubricating oil additive.