Wire rod for piston rod of automobile shock absorber and production method of wire rod

Through the production method combining LF refining and VD vacuum treatment, chemical elements and process flow are optimized and the grinding process is cancelled, which solves the problems of high cost of traditional strip processing and severe surface quality requirements, and achieves high-quality and low-cost automotive shock absorption The piston rod is produced with coil strips, which meets the needs of high surface quality and low cost.

CN118996255APending Publication Date: 2024-11-22LIANFENG STEEL (ZHANGJIAGANG) CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411090117.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

There is a grinding process in the processing process of traditional automotive shock absorbers for piston rods, resulting in high material loss, high cost and strict surface quality requirements, making it difficult to meet the dual needs of high quality and low cost.

Method used

Using a production method combining LF refining and VD vacuum treatment, optimize chemical element components and production process flow, cancel the grinding process, and through converter smelting, continuous casting, billet finishing, controlled rolling and cold-controlled and refined packaging, ensuring that the strips are being pulled After extraction, it can directly meet the eddy current flaw detection requirements.

Benefits of technology

It significantly improves the surface quality and mechanical properties of the strips, reduces processing costs, simplifies production processes, improves production efficiency, and reduces waste and energy consumption, in line with environmental protection and sustainable development goals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996255A_ABST
    Figure CN118996255A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wire rod production, and provides a wire rod for an automobile shock absorber piston rod and a production method of the wire rod, and the surface quality of the wire rod is remarkably improved by accurately adjusting the proportion of chemical elements and improving the production process. The new technology meets the requirement of direct eddy current flaw detection after the wire rod is drawn, so that the grinding procedure is omitted, and the production cost is effectively reduced. Key technologies include double refining treatment, continuous casting billet finishing, controlled rolling and controlled cooling technologies and refined packaging processes, and stability and reliability of product quality are guaranteed. The wire rod has the characteristics of less macrostructure looseness, good inclusion control, shallow decarburized layer and excellent mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wire rod production, and in particular to a wire rod for a piston rod of an automobile shock absorber and a production method thereof. Background Art

[0002] Automobile shock absorbers are composed of a piston rod, a cylinder body, and a spring. The shock absorber cylinder is filled with high-pressure hydraulic oil or gas. If the piston rod has surface defects such as pits and pitting, it will cause oil leakage, air leakage, or even breakage, resulting in failure of the shock absorber. Therefore, shock absorber manufacturers have strict requirements on the surface quality of the piston.

[0003] Wire rods for automobile shock absorber piston rods are usually made of medium carbon steel, such as S35C, S45C, 45 steel, etc. Due to the strict surface quality requirements of shock absorber piston rods, the traditional processing technology is wire rod, drawing, grinding (single-side grinding of about 1mm), and eddy current flaw detection. The grinding process increases material loss, reduces production efficiency, and increases processing costs.

[0004] As competition in the automobile industry intensifies, in order to reduce processing costs, it is required to cancel the grinding process so as to reduce the processing cost of wire rods for automobile shock absorber piston rods. In order to meet the dual needs of high surface quality and low processing cost, the present invention provides a wire rod for automobile shock absorber piston rods and a production method thereof. Summary of the invention

[0005] The present invention develops a wire rod for an automobile shock absorber piston rod, thereby improving the surface quality of the wire rod for the automobile shock absorber piston rod, meeting the requirement of directly performing eddy current flaw detection on the wire rod for the automobile shock absorber piston rod after drawing, eliminating the grinding process, and reducing the processing cost of the wire rod for the automobile shock absorber piston rod.

[0006] In a first aspect, the present invention provides a wire rod for a piston rod of an automobile shock absorber, comprising: the chemical element composition of the wire rod is as follows by weight percentage: chemical composition: C 0.40-0.48%, Si 0.15-0.35%, Mn 0.50-1.00%, P≤0.015%, S≥0.010%, Ni≤0.20%, Cu≤0.20%, Mo≤0.10%, N≤0.0060%, O≤0.0015%, and also contains one or more of Cr 0.05-0.25%, Al 0.005-0.035%, Ti 0.02-0.05%, B 0.0008-0.0035%, and the rest is Fe and unavoidable impurities.

[0007] In a second aspect, the present invention provides a method for producing a wire rod for a piston rod of an automobile shock absorber, which is applied to produce the wire rod for the piston rod of an automobile shock absorber, and comprises the following steps:

[0008] Step S1: converter smelting, in which the steel is smelted in a converter, the raw materials are melted into molten steel through high-temperature smelting, and impurities therein are removed;

[0009] Step S2: LF refining, transferring the molten steel smelted in the converter to the LF refining furnace for refining. In the LF refining step, alloy elements are added and the chemical composition of the molten steel is adjusted to improve the purity and performance of the steel.

[0010] Step S3: VD vacuum treatment. The molten steel after LF refining will be sent to the VD vacuum treatment equipment. In a vacuum environment, the gas and inclusions in the molten steel are further removed to ensure the purity and quality of the steel.

[0011] Step S4: Continuous casting: The molten steel after vacuum treatment will be cast into continuous casting billets; this step requires strict control of the casting temperature and speed to ensure the internal quality and surface quality of the continuous casting billets.

[0012] Step S5: Billet finishing: After the continuous casting billet is cooled, the billet is subjected to a finishing treatment, and the finishing process includes full peeling and magnetic particle inspection to remove surface defects and internal cracks, thereby ensuring the surface and internal quality of the billet.

[0013] Step S6: Heating: The finished billet will be sent to a heating furnace for uniform heating to prepare for the subsequent rolling process.

[0014] Step S7: controlled rolling and controlled cooling: the heated billet enters the rolling mill for rolling. The rolling temperature and rolling speed of the rolling mill are controlled according to the preset rolling temperature and rolling speed to form wire rods of required specifications. After rolling, the wire rods are subjected to fine cooling treatment to obtain cooled wire rods.

[0015] The heated billet will enter the rolling mill for rolling to form the required specifications of the wire rod. During the rolling process, the rolling temperature and rolling speed are controlled to obtain the ideal organizational structure and mechanical properties. After rolling, the wire rod will undergo a fine cooling treatment to reduce the thickness of the iron oxide scale and improve the density of the iron oxide scale.

[0016] Furthermore, the method for producing the wire rod for the automobile shock absorber piston rod provided by the present invention further comprises the following steps:

[0017] Step S8: Inspection: The cooled wire rod is subjected to quality inspection, which includes the inspection of surface quality, dimensional accuracy, chemical composition and mechanical properties to ensure that the product meets relevant standards and customer requirements.

[0018] Step S9: Packaging: The qualified wire rods will be packaged to obtain packaged wire rods. During the packaging process, fine operations are taken to ensure that the packaging temperature and packaging pressure are appropriate to avoid damage to the wire rods. At the same time, anti-scratch lubricant is sprayed on the surface of the wire rod to protect the wire rod from damage during transportation and storage.

[0019] Step S10: Weighing, marking and warehousing: Finally, the packaged wire rods are weighed, marked, and classified and stored according to specifications and batches to facilitate subsequent sales and shipment.

[0020] Furthermore, the method for producing the wire rod for the automobile shock absorber piston rod provided by the present invention further comprises the following steps:

[0021] LF refining, which further adjusts the chemical composition of the molten steel by heating, stirring and adding alloys, and removes impurities in the process, is used to reduce small particle inclusions in the molten steel and improve the purity of the steel;

[0022] VD vacuum treatment further treats the molten steel after LF refining. By vacuumizing to reduce the ambient pressure, the dissolved gases and inclusions in the molten steel are more easily released from the molten steel, which is used to improve the purity of the steel and remove large particle inclusions.

[0023] The combined use of these two refining steps enables the large particle inclusions in the molten steel to be removed more effectively, thereby improving the overall quality of the steel. In this way, LF+VD double refining provides strong technical support for the production of high-quality and high-performance steel.

[0024] Furthermore, the method for producing a wire rod for a piston rod of an automobile shock absorber provided by the present invention comprises, in step S7, the following steps:

[0025] After rolling, the wire rod enters the controlled cooling stage and adopts a delayed cooling mode. The spinning temperature is controlled at 750-800℃. During the cooling process, the insulation cover remains fully open and the first fan is opened at 50%.

[0026] Furthermore, the method for producing a wire rod for a piston rod of an automobile shock absorber provided by the present invention comprises, in step S9, the following steps:

[0027] Control packaging temperature: packaging temperature ≤50℃;

[0028] Precise adjustment of packing pressure: the packing pressure can be set between 10 and 14 tons;

[0029] Spray anti-scratch lubricant on the surface of the wire rod: Before packaging, spray a layer of anti-scratch lubricant on the surface of the wire rod.

[0030] The beneficial effects of the present invention are as follows:

[0031] Improved surface quality: By optimizing the chemical composition and the entire production process, the surface quality of the wire rod for automobile shock absorber piston rods has been significantly improved. This quality improvement allows the wire rod to directly meet the requirements of eddy current testing after drawing, thus eliminating the grinding process and simplifying the production process.

[0032] Reduce processing costs: The elimination of the grinding process not only improves production efficiency, but also significantly reduces the processing cost of wire rods for automobile shock absorber piston rods. In addition, by optimizing the controlled rolling and cooling process and the packaging process, the utilization rate of materials is further improved, the scrap rate is reduced, and the overall cost is also reduced.

[0033] Refined production and quality control: The present invention realizes all-round refined control of the production process through LF+VD double refining, strict control of continuous casting process, billet finishing, controlled rolling and cooling, and refined packaging, thereby ensuring the stability and reliability of product quality.

[0034] Environmentally friendly: By optimizing the production process, the waste and energy consumption generated by the grinding process are reduced, which is in line with the current high attention to environmental protection and sustainable development.

[0035] Broad application prospects: Due to the improvement of product quality and the reduction of cost, the wire rod provided by the present invention has a broader market prospect in the field of automobile shock absorber piston rod manufacturing and other similar application fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the technical solution of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0037] Figure 1 A schematic diagram of a method flow chart provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The technical solutions provided by the embodiments of the present invention are described in detail below in conjunction with the drawings.

[0039] The method of the invention effectively improves the surface quality of the wire rod for the automobile shock absorber piston rod. The wire rod for the automobile shock absorber piston rod is directly subjected to eddy current flaw detection without grinding after being drawn, thereby reducing the grinding process and reducing the production cost.

[0040] In a first aspect, the present invention provides a wire rod for a piston rod of an automobile shock absorber, comprising: the chemical element composition of the wire rod is as follows by weight percentage: chemical composition: C 0.40-0.48%, Si 0.15-0.35%, Mn 0.50-1.00%, P≤0.015%, S≥0.010%, Ni≤0.20%, Cu≤0.20%, Mo≤0.10%, N≤0.0060%, O≤0.0015%, and also contains one or more of Cr 0.05-0.25%, Al 0.005-0.035%, Ti 0.02-0.05%, B 0.0008-0.0035%, and the rest is Fe and unavoidable impurities.

[0041] C (Carbon): Mainly affects the strength and hardness of steel, ensuring that the wire rod has sufficient strength and hardness while maintaining good machinability.

[0042] Si (Silicon): Improves the strength and hardness of steel, improves the steel's oxidation resistance and heat resistance, and helps to improve the overall performance of wire rod.

[0043] Mn (Manganese): As a deoxidizer and desulfurizer, it reduces the oxygen and sulfur content in steel, increases the strength and hardness of steel, improves the hardenability of steel, and ensures the quality of wire rod.

[0044] P (phosphorus) and S (sulfur): These two elements are generally regarded as harmful elements in steel and their content should be reduced as much as possible to avoid brittleness problems caused.

[0045] Ni (nickel): Improves the strength, toughness and corrosion resistance of steel, but the content is limited to maintain the dominant role of other elements.

[0046] Cu (Copper): Improves the corrosion resistance and antibacterial properties of steel, but excessive copper can cause hot brittleness of steel, so the content is limited.

[0047] Mo (molybdenum): Improves the strength, hardness and corrosion resistance of steel and helps improve the overall performance of wire rod.

[0048] N (nitrogen): One of the factors that affect the toughness of steel. Too high nitrogen content will lead to a decrease in the toughness of steel, so the content is strictly limited.

[0049] O (oxygen): A harmful element in steel that increases its brittleness, so its content is limited to maintain the purity and performance of the steel.

[0050] Cr (Chromium): Improves the hardness, wear resistance and corrosion resistance of steel, and helps improve the surface quality and durability of wire rods.

[0051] Al (Aluminum): As a deoxidizer, it removes oxygen from steel, improves the strength of steel and refines grains, helping to maintain stable performance of steel.

[0052] Ti (titanium): combines with harmful elements in steel to improve the purity and performance of steel and help reduce harmful inclusions in steel.

[0053] B (boron): micro-alloying element that improves the hardenability and strength of steel and helps optimize the mechanical properties of wire rod.

[0054] The chemical elements of the invention improve the surface quality, mechanical properties and processing properties of the wire rod for the automobile shock absorber piston rod through precise proportioning and synergistic effect.

[0055] In a second aspect, the present invention provides a method for producing a wire rod for a piston rod of an automobile shock absorber, which is applied to produce the wire rod for the piston rod of an automobile shock absorber, and comprises the following steps:

[0056] Step S1: converter smelting, in which the steel is smelted in a converter, the raw materials are melted into molten steel through high-temperature smelting, and impurities therein are removed;

[0057] Step S2: LF refining, transferring the molten steel smelted in the converter to the LF refining furnace for refining. In the LF refining step, alloy elements are added and the chemical composition of the molten steel is adjusted to improve the purity and performance of the steel.

[0058] Step S3: VD vacuum treatment. The molten steel after LF refining will be sent to the VD vacuum treatment equipment. In a vacuum environment, the gas and inclusions in the molten steel are further removed to ensure the purity and quality of the steel.

[0059] Step S4: Continuous casting: The molten steel after vacuum treatment will be cast into continuous casting billets; this step requires strict control of the casting temperature and speed to ensure the internal quality and surface quality of the continuous casting billets.

[0060] Step S5: Billet finishing: After the continuous casting billet is cooled, the billet is subjected to finishing treatment, and the finishing process includes full peeling and magnetic particle inspection to remove surface defects and internal cracks to ensure the surface and internal quality of the billet.

[0061] Step S6: Heating: The finished billet will be sent to a heating furnace for uniform heating to prepare for the subsequent rolling process.

[0062] Step S7: controlled rolling and controlled cooling: the heated billet enters the rolling mill for rolling. The rolling temperature and rolling speed of the rolling mill are controlled according to the preset rolling temperature and rolling speed to form wire rods of required specifications. After rolling, the wire rods are subjected to fine cooling treatment to obtain cooled wire rods.

[0063] The heated billet will enter the rolling mill for rolling to form the required specifications of the wire rod. During the rolling process, the rolling temperature and rolling speed are controlled to obtain the ideal organizational structure and mechanical properties. After rolling, the wire rod will undergo a fine cooling treatment to reduce the thickness of the iron oxide scale and improve the density of the iron oxide scale.

[0064] Furthermore, the method for producing the wire rod for the automobile shock absorber piston rod provided by the present invention further comprises the following steps:

[0065] Step S8: Inspection: The cooled wire rod is subjected to quality inspection, which includes the inspection of surface quality, dimensional accuracy, chemical composition and mechanical properties to ensure that the product meets relevant standards and customer requirements.

[0066] Step S9: Packaging: The qualified wire rods will be packaged to obtain packaged wire rods. During the packaging process, fine operations are taken to ensure that the packaging temperature and packaging pressure are appropriate to avoid damage to the wire rods. At the same time, anti-scratch lubricant is sprayed on the surface of the wire rod to protect the wire rod from damage during transportation and storage.

[0067] Step S10: Weighing, marking and warehousing: Finally, the packaged wire rods are weighed, marked, and classified and stored according to specifications and batches to facilitate subsequent sales and shipment.

[0068] Furthermore, the method for producing the wire rod for the automobile shock absorber piston rod provided by the present invention further comprises the following steps:

[0069] LF refining, which further adjusts the chemical composition of the molten steel by heating, stirring and adding alloys, and removes impurities in the process, is used to reduce small particle inclusions in the molten steel and improve the purity of the steel;

[0070] VD vacuum treatment further treats the molten steel after LF refining. By vacuumizing to reduce the ambient pressure, the dissolved gases and inclusions in the molten steel are more easily released from the molten steel, which is used to improve the purity of the steel and remove large particle inclusions.

[0071] The combined use of these two refining steps enables the large particle inclusions in the molten steel to be removed more effectively, thereby improving the overall quality of the steel. In this way, LF+VD double refining provides strong technical support for the production of high-quality and high-performance steel.

[0072] In the process of producing wire rod for automobile shock absorber piston rod, the specific process, effects and collaborative working principle of LF refining and VD vacuum treatment are as follows:

[0073] LF refining: Specific process: The molten steel smelted in the converter is transferred to the LF refining furnace with heating, stirring and alloying functions. By adding alloying elements (such as chromium, aluminum, titanium, boron, etc.), the chemical composition of the molten steel is further adjusted to the target requirements. At the same time, small particle inclusions and other impurities are removed by heating and stirring. The effects brought include precise adjustment of chemical composition, significant improvement of molten steel purity, and improvement of mechanical properties and surface quality of steel.

[0074] VD vacuum treatment: Specific process: The molten steel after LF refining is sent to the VD vacuum treatment equipment, which reduces the ambient pressure in a vacuum environment, making it easier for dissolved gases and inclusions to be released from the molten steel. In addition, it can effectively remove harmful gases such as hydrogen, significantly remove gases and inclusions, especially hydrogen, and further improve the purity and overall quality of the steel.

[0075] Principle of collaborative working: LF refining provides a high-quality molten steel foundation for subsequent VD vacuum treatment. Through preliminary chemical adjustment and impurity removal, VD treatment is made more efficient.

[0076] VD vacuum treatment, based on LF refining, uses a vacuum environment to further purify molten steel, especially to remove large particle inclusions and harmful gases, significantly improving the purity and performance of the steel.

[0077] The combination of these two steps not only improves the purity of the steel, but also greatly improves the mechanical properties and surface quality of the steel, thereby meeting the high quality requirements of the wire rod for the automobile shock absorber piston rod. By eliminating the grinding process, the present invention also reduces the processing cost.

[0078] Furthermore, the method for producing a wire rod for a piston rod of an automobile shock absorber provided by the present invention comprises, in step S7, the following steps:

[0079] After rolling, the wire rod enters the controlled cooling stage and adopts a delayed cooling mode. The spinning temperature is controlled at 750-800℃. During the cooling process, the insulation cover remains fully open and the first fan is opened at 50%.

[0080] Furthermore, the method for producing a wire rod for a piston rod of an automobile shock absorber provided by the present invention comprises, in step S9, the following steps:

[0081] Control packaging temperature: packaging temperature ≤50℃;

[0082] Precise adjustment of packing pressure: the packing pressure can be set between 10 and 14 tons;

[0083] Spray anti-scratch lubricant on the surface of the wire rod: Before packaging, spray a layer of anti-scratch lubricant on the surface of the wire rod.

[0084] The functions and effects of each step of the method for producing a wire rod for a piston rod of an automobile shock absorber provided by the present invention are as follows:

[0085] Converter smelting: This step melts the raw materials into molten steel through high temperature and preliminarily removes impurities, providing good quality starting materials for subsequent steps.

[0086] LF refining: In this step, impurities in the molten steel are further removed by adding alloying elements and adjusting the chemical composition of the molten steel, thereby improving the purity and overall performance of the steel.

[0087] VD vacuum treatment: With the help of vacuum environment, this step removes gases and inclusions in the molten steel more deeply, significantly improving the purity and mechanical properties of the steel.

[0088] Continuous casting: Molten steel is precisely cast into continuous casting billets, and the temperature and speed are strictly controlled to ensure its internal and external quality. This is a key step in steel forming.

[0089] Billet finishing: Remove surface defects and internal cracks of billets through full peeling and magnetic particle inspection to provide high-quality raw materials for subsequent processing.

[0090] Heating: Prepares for the rolling process by uniformly heating the steel to ensure uniform deformation during rolling.

[0091] Controlled rolling and controlled cooling: In this step, the steel is precisely rolled into wire rods of the required specifications and subjected to a fine cooling treatment to improve its mechanical properties and dimensional accuracy.

[0092] Inspection: Comprehensive quality inspection ensures that products meet various standards and customer requirements and is an important part of product quality control.

[0093] Packaging: Qualified products are packaged, and the temperature and pressure are strictly controlled during the process. Anti-scratch lubricant is sprayed to protect the wire rod from damage during transportation and storage.

[0094] Weighing, Labeling and Warehousing: Finally, the products are weighed, labeled and sorted into warehouses, ready for sale and shipment.

[0095] During the packaging step, precise control of temperature and pressure, as well as spraying of anti-galling lubricant are critical operations to ensure the safety and quality of the wire rods used for automotive shock absorber piston rods during transportation and storage.

[0096] First of all, the control of packaging temperature is mainly to prevent the wire rod from being deformed or generating thermal stress concentration due to excessive temperature, which will affect the dimensional accuracy and surface quality of the wire rod. By maintaining the packaging temperature below 50℃, the wire rod can be effectively prevented from being deformed due to thermal stress, ensuring that its dimensional accuracy and original shape are not affected.

[0097] Secondly, the control of packing pressure is to ensure that the wire rod is tightly packed while avoiding damage to the wire rod such as indentation and deformation caused by excessive pressure. The packing pressure is set within the range of 10 to 14 tons, which not only ensures the tightness of the wire rod, but also prevents damage caused by excessive pressure.

[0098] Finally, the purpose of spraying anti-scratch lubricant is to form a protective film on the surface of the wire rod to reduce scratches and damage caused by friction during packaging, transportation and storage. This protective film not only reduces the direct contact and friction between the wire rods, but also isolates air and moisture to a certain extent, thereby slowing down the oxidation and corrosion of the wire rod surface.

[0099] The present invention achieves the technical effects of improving the surface quality of the wire rod for the automobile shock absorber piston rod, meeting the requirement of directly performing eddy current flaw detection after drawing, eliminating the grinding process and reducing the processing cost through the following technical steps.

[0100] Optimize chemical element composition: Through specific chemical element ratios, including C, Si, Mn, etc., and add elements such as Cr, Al, Ti, B, etc., to optimize the overall performance of the material.

[0101] Refining and vacuum treatment: LF refining and VD vacuum treatment technology are used to effectively remove impurities and gases in molten steel, thereby improving the purity and quality of steel.

[0102] Continuous casting and billet finishing: The continuous casting process ensures the internal and external quality of the billet, and the subsequent finishing treatment further eliminates surface defects and internal cracks.

[0103] Controlled rolling and controlled cooling technology: When rolling wire rods, the rolling temperature and speed are controlled, as well as the subsequent cooling treatment, which helps to improve the mechanical properties and surface quality of the wire rods.

[0104] Strict quality inspection and refined packaging: All wire rods undergo comprehensive quality inspection and refined operations are adopted during the packaging process to ensure the integrity and quality of the product.

[0105] The quality inspection part is the key link to ensure that the quality and performance of the wire rod for automobile shock absorber piston rod meet the standards. The following are the specific inspection standards and processes:

[0106] Surface quality: Check whether there are pits, pits, cracks and other defects on the surface of the wire rod. The depth of these defects should not exceed 0.05mm. At the same time, the thickness of the iron oxide scale should not exceed 20 microns.

[0107] Dimensional accuracy: The diameter, length and other dimensions of the wire rod must meet the specification requirements.

[0108] Chemical composition: The composition test must comply with the prescribed chemical element ratio, such as C 0.400.48%, Si0.150.35%, etc.

[0109] Mechanical properties: Tensile strength must reach or exceed 600MPa, and other properties such as yield strength and elongation should also meet the standards.

[0110] Inclusions and decarburization layer: The inclusion fineness must be lower than level 4.5, and the total decarburization layer depth must not exceed 0.7%D.

[0111] The specific testing process is as follows;

[0112] Preliminary inspection: Preliminary inspection of the appearance of the wire rod after cooling.

[0113] Size measurement: Use professional tools to measure.

[0114] Chemical composition analysis: Spectral analysis and other methods are used to detect element content.

[0115] Mechanical performance test: Conduct tensile tests and other tests to test mechanical performance indicators.

[0116] Inclusion and decarburization layer detection: Use a microscope or other equipment to observe the internal conditions.

[0117] Eddy current testing: detects tiny internal cracks and defects.

[0118] To ensure product quality and performance, we take the following measures: strict production process control, use of advanced testing equipment, establishment of a comprehensive quality inspection process, and formulation of standardized operation and management specifications. These measures together ensure that products meet standards and meet customer needs.

[0119] The present invention significantly improves the surface quality of the wire rod, enabling it to meet the standard of direct eddy current flaw detection after drawing, thereby eliminating the grinding process. This not only simplifies the production process, but also reduces the processing cost.

[0120] The wire rod for automobile shock absorber of the present invention has low-power general looseness, central looseness and ingot-shaped segregation ≤0.5 level; inclusion A+B+C+D fine system ≤4.5 level, DS ≤1.5 level; total decarburization layer depth ≤0.7%D; tensile strength ≥600MPa, iron oxide thickness ≤20 microns, surface defect depth ≤0.05mm, meeting customers' requirements for high surface quality, and customers' eddy current flaw detection pass rate after drawing ≥97%.

[0121] The technology of the present invention has shown significant advantages and innovations in many aspects.

[0122] First, from the perspective of production efficiency, the elimination of the grinding process has greatly improved production efficiency. This improvement not only shortens the production cycle, but also reduces costs. Specifically, the elimination of the grinding process reduces material loss, thereby reducing production costs. At the same time, the improvement in processing efficiency also speeds up production.

[0123] Secondly, in terms of product quality, the surface quality and mechanical properties of the technology of the present invention are significantly better than those of the prior art. The looseness of the macrostructure is less, the inclusions are properly controlled, and the decarburization layer is shallow, all of which make the performance of the product more stable and reliable. In addition, the high standard of tensile strength also ensures the durability of the product.

[0124] Furthermore, the present invention achieves the goal of environmental protection and sustainable development by optimizing the production process. The reduction of grinding steps not only reduces waste generation, but also reduces energy consumption, which is in line with the current concept of environmental protection and sustainable development.

[0125] In general, compared with the prior art, the present invention has significant advantages in surface quality, mechanical properties, production efficiency, cost control and environmental protection, etc. These innovations make the present invention have extremely high practical value and application prospects in the production of wire rods for automobile shock absorber piston rods.

[0126] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A wire rod for a piston rod of an automobile shock absorber, characterized in that: include: The chemical element composition of the wire rod is as follows by weight percentage: chemical composition: C 0.40-0.48%, Si 0.15-0.35%, Mn 0.50-1.00%, P≤0.015%, S≥0.010%, Ni≤0.20%, Cu≤0.20%, Mo≤0.10%, N≤0.0060%, O≤0.0015%, and also contains one or more of Cr0.05-0.25%, Al 0.005-0.035%, Ti 0.02-0.05%, B 0.0008-0.0035%, and the rest is Fe and unavoidable impurities.

2. A method for producing a wire rod for a piston rod of an automobile shock absorber, which is applied to produce the wire rod for a piston rod of an automobile shock absorber as claimed in claim 1, characterized in that: The steps include: Step S1: converter smelting, in which the steel is smelted in a converter, the raw materials are melted into molten steel through high-temperature smelting, and impurities therein are removed; Step S2: LF refining, transferring the molten steel smelted in the converter to the LF refining furnace for refining. In the LF refining step, alloy elements are added and the chemical composition of the molten steel is adjusted; Step S3: VD vacuum treatment: the molten steel after LF refining will be sent to VD vacuum treatment equipment to further remove gas and inclusions in the molten steel under vacuum environment; Step S4: continuous casting: the molten steel after vacuum treatment will be cast into continuous casting billets; Step S5: Steel billet finishing: After the continuous casting billet is cooled, the steel billet is subjected to finishing treatment, and the finishing treatment process includes full peeling and magnetic particle inspection to remove surface defects and internal cracks; Step S6: Heating: The finished billet will be sent to a heating furnace for uniform heating; Step S7: controlled rolling and controlled cooling: the heated billet enters the rolling mill for rolling. The rolling temperature and rolling speed of the rolling mill are controlled according to the preset rolling temperature and rolling speed to form wire rods of required specifications. After rolling, the wire rods are subjected to fine cooling treatment to obtain cooled wire rods.

3. The method for producing a wire rod for a piston rod of an automobile shock absorber according to claim 2, characterized in that: The following steps are also included; Step S8: Inspection: Performing quality inspection on the cooled wire rod, the quality inspection includes the inspection of surface quality, dimensional accuracy, chemical composition and mechanical properties; Step S9: Packaging: The qualified wire rods will be packaged to obtain packaged wire rods; Step S10: Weighing, marking and storage: Finally, the packaged wire rods are weighed, marked, and classified and stored according to specifications and batches.

4. The method for producing a wire rod for a piston rod of an automobile shock absorber according to claim 2, characterized in that: The following steps are also included; LF refining, which further adjusts the chemical composition of the molten steel by heating, stirring and adding alloys, and removes impurities in the process, is used to reduce small particle inclusions in the molten steel and improve the purity of the steel; VD vacuum treatment further treats the molten steel after LF refining. By vacuumizing to reduce the ambient pressure, the dissolved gases and inclusions in the molten steel are more easily released from the molten steel, which is used to improve the purity of the steel and remove large particle inclusions.

5. The method for producing a wire rod for a piston rod of an automobile shock absorber according to claim 2, characterized in that: In step S7, The steps include: The rolled wire rod enters the controlled cooling stage and adopts a delayed cooling mode. The spinning temperature is controlled at 750-800℃. During the cooling process, the insulation cover remains fully open and the first fan is opened at 50%.

6. The method for producing a wire rod for a piston rod of an automobile shock absorber according to claim 2, characterized in that: In step S9, the following steps are included: Control packaging temperature: packaging temperature ≤50℃; Precise adjustment of packing pressure: the packing pressure can be set between 10 and 14 tons; Spray anti-scratch lubricant on the surface of the wire rod: Before packaging, spray a layer of anti-scratch lubricant on the surface of the wire rod.

Citation Information

Cited By

  • Large-specification wire rod, preparation method thereof and air cooling device

    CN121491135A