Al2O3 modified YSZ composite thermal barrier coating resistant to high-temperature CMAS corrosion and preparation method of Al2O3 modified YSZ composite thermal barrier coating

By introducing Al2O3 modification into the YSZ thermal barrier coating, Al2O3-YSZ composite coating is formed, which solves the sensitivity of YSZ coating to CMAS corrosion at high temperatures, and achieves higher high-temperature stability and thermal insulation effect. Extend the service life of the coating.

CN118996344APending Publication Date: 2024-11-22BEIHANG UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411092228.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

YSZ thermal barrier coatings are susceptible to CMAS corrosion during high-temperature service, resulting in structural damage and degradation of performance. It is difficult for existing materials to effectively resist CMAS infiltration and corrosion at high temperatures.

Method used

The YSZ composite thermal barrier coating was used to modify the Al2O3 YSZ composite thermal barrier coating, including forming a metal bonding layer and composite ceramic structural coating on the high-temperature alloy matrix. The YSZ and Al2O3-YSZ bilayer structures were prepared by electron beam physical vapor deposition, with the Al2O3 content of 20wt. % to 30 wt.%, to improve the high temperature stability of the coating and its resistance to CMAS corrosion.

Benefits of technology

The coating is dense in structure and has low thermal conductivity, which can effectively prevent CMAS from penetrating, extend the high-temperature service life of the coating, and maintain structural integrity above 1300°C, reduce the difference in thermal expansion coefficient of the coating, improve binding force, and enhance isolation Thermal effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996344A_ABST
    Figure CN118996344A_ABST
Patent Text Reader

Abstract

The invention provides an Al2O3 modified YSZ composite thermal barrier coating resistant to high-temperature CMAS corrosion and a preparation method of the Al2O3 modified YSZ composite thermal barrier coating. The composite thermal barrier coating comprises a metal bonding layer and a composite ceramic structure coating which are arranged on a high-temperature alloy matrix, wherein the composite ceramic structure coating comprises a first ceramic layer (YSZ layer) located on the inner side and a second ceramic layer (Al2O3 modified YSZ (AYSZ) layer) located on the outer side. The composite thermal barrier coating provided by the invention is compact in structure and low in thermal conductivity, has relatively good high-temperature phase stability, and can effectively prevent permeation of molten CMAS. Under the conditions that the high temperature is 1300 DEG C or above and molten CMAS corrosion exists, the bottom of the AYSZ layer of the coating and the YSZ layer can still keep structural integrity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal barrier coatings, and in particular to an Al2O3-modified YSZ composite thermal barrier coating resistant to high-temperature CMAS corrosion and a preparation method thereof. Background Art

[0002] Thermal barrier coating is a thermal protection technology that coats high-temperature resistant, heat-insulating and corrosion-resistant ceramic materials on the surface of an alloy substrate to reduce the temperature of the metal substrate. It is one of the three key technologies in the high-temperature field of advanced aero-engines, along with high-temperature alloy technology and high-efficiency air cooling technology.

[0003] The most widely used ceramic insulation material for engine service is 6-8wt% yttria-stabilized zirconia (YSZ). The melting point of YSZ material is ~2600℃, the thermal conductivity is ~2.2W / m·K at 1200℃, and the thermal expansion coefficient is ~10.5×10 -6 K -1 ; Elastic modulus ~60GPa; Hardness ~21GPa; Fracture toughness ~4.1MPa·m 1 / 2 . When the service temperature of the YSZ coating exceeds 1200℃, the metastable tetragonal phase in the coating will undergo a phase change, resulting in severe sintering of the coating, causing the structural integrity of the original coating to be destroyed, the thermodynamic properties to decrease, and its service performance to be affected. In addition, as the temperature of aircraft engines continues to increase, the thermal barrier coating of the engine blades is susceptible to corrosion during high-temperature service by a silicate environmental deposit whose main component is CaO-MgO-Al2O3-SiO2 (CMAS). This CMAS deposit has a melting point of about 1200℃ and is molten at high temperatures. It adheres to the surface of the blade thermal barrier coating, infiltrates, spreads, and penetrates into the coating through the pores and microcracks of the coating. For the YSZ coating, on the one hand, due to the large amount of CaO in the molten CMAS, 2+ and Mg 2+ As a stabilizer of ZrO2, it dissolves into the YSZ lattice and replaces Y 3+The effect of CMAS causes the formation of Y-poor areas, resulting in the destruction of the original YSZ stable structure. Other components in CMAS are also prone to thermochemical reactions with YSZ, resulting in phase changes, causing the YSZ coating to fail. On the other hand, the infiltration of CMAS blocks the air film cooling holes and generates large shrinkage stresses during the solidification process, causing thermal mismatch inside the ceramic layer, reduced strain tolerance, and increased cracks inside the coating, which leads to delamination and cracking of the coating and layer-by-layer peeling failure. (See reference 1: NPBansal, SRChoi., Ceramics International, 2015, 41(3): 3901-3909.) At present, the materials used to resist CMAS corrosion are mainly divided into three types of protective coatings: dense, sacrificial, and anti-wetting. In particular, for YSZ coatings prepared by electron beam physical vapor deposition (EB-PVD), although this method can obtain thermal barrier coatings with good bonding strength and long service life, due to the special columnar structure of the coating, the gaps between the columns easily become channels for the flow and infiltration of molten CMAS, causing damage to the YSZ coating structure. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes an Al2O3 modified YSZ composite thermal barrier coating resistant to high-temperature CMAS corrosion and a preparation method thereof, so as to alleviate the CMAS corrosion problem in the high-temperature / ultra-high-temperature thermal barrier coating service environment, and further improve the high-temperature stability of the coating and extend the service life of the coating.

[0005] According to the first aspect, an Al2O3 modified YSZ composite thermal barrier coating resistant to high-temperature CMAS corrosion is proposed, characterized in that it includes a metal bonding layer and a composite ceramic structural coating on a high-temperature alloy substrate, wherein the composite ceramic structural coating refers to a first ceramic layer (YSZ layer) located on the inner side and a second ceramic layer (Al2O3 modified YSZ (AYSZ) layer) located on the outer side.

[0006] In some embodiments, the first ceramic layer (YSZ layer) is deposited by electron beam evaporation of a YSZ target (8wt.% Y2O3-Zr2O) with a thickness of 100-125μm. The second ceramic layer (AYSZ layer) is made by electron beam bombardment of a self-made Al2O3-YSZ composite target, with an Al2O3 content of 20wt.% to 30wt.% of the AYSZ composite coating, and the AYSZ layer thickness is 45-75μm. The total thickness of the composite ceramic structure coating does not exceed 200μm.

[0007] In some embodiments, the metal bonding layer includes one of the following three materials: the first is NiCrAlYSi, whose components include 40-60wt.% Ni, 14-28wt.% Cr, 15-20wt.% Al, 0.05-2wt.% Y and 0.05-2wt.% Si; the second is NiAlX, X is any one of Hf, Zr, Dy, and Y, and its components include 40-60wt.% Ni, 36-60wt.% Al, and 0.05-2wt.% X; the third is NiPtAl, whose components include 40-60mol.% Ni, 18-22mol.% Pt, and 30-45mol.% Al.

[0008] In some embodiments, the thickness of the metal bonding layer is 30-60 μm.

[0009] According to the second aspect, a method for preparing an Al2O3-modified YSZ composite thermal barrier coating resistant to high temperature CMAS corrosion is provided, the method comprising the following steps:

[0010] The first step is the pretreatment of high temperature alloy;

[0011] The second step is to prepare a metal bonding layer on the surface of the high-temperature alloy. After the metal bonding layer is prepared, the alloy is taken out and placed in a vacuum annealing furnace for vacuum heat treatment. The heat treatment temperature is set at 1050-1150°C, the time is 2-4h, and the vacuum degree is set at 7-9×10 -5 mbar, cooled in the furnace and taken out at room temperature;

[0012] In the third step, a ceramic coating is prepared on the surface of the metal bonding layer by electron beam physical vapor deposition. The preparation process includes: placing the sample to be evaporated on the electron beam physical vapor deposition rotating substrate, placing the target material to be evaporated in the electron beam physical deposition crucible, and setting the vacuum degree of the deposition chamber to 10 -3 Pa, the substrate is preheated to 900-980°C, the oxygen flux is set to 100-105sccm, the voltage is controlled to 18-19kV, the rotation speed of the sample substrate is controlled to be constant at 15rpm, and the target rotation speed is 0.8r / min; the YSZ coating is preferentially deposited on the surface of the metal bonding layer, the YSZ target is selected, the electron beam current is 0.65-0.76A, and the deposition time is 35-45min, and a YSZ layer of 100-125μm can be obtained; then the AYSZ layer is deposited on the surface of the YSZ layer, the Al2O3-YSZ composite target (AYSZ target) is selected, the electron beam current is 0.69-0.73A, and the deposition time is 20-22min, and a 45-75μm AYSZ layer is obtained.

[0013] In some embodiments, the Al2O3-YSZ composite target in the third step is obtained by digging a columnar hole of a certain size at the bottom of the columnar YSZ target, and then placing an Al2O3 target of the same size in the hole; when the electron beam evaporates, the composite target is inverted, and the electron beam gun excites the junction of the YSZ target and the Al2O3 target, so that the ratio of Al2O3 and YSZ components in the AYSZ coating can be controlled by changing the position of the electron beam gun.

[0014] In some embodiments, the second step adopts any one of the following three methods to prepare the metal bonding layer: preparing a NiCrAlYSi bonding layer by multi-arc ion plating; preparing a NiAlX bonding layer by electron beam physical vapor deposition; preparing a NiPtAl metal bonding layer by electroplating and embedding.

[0015] In some more specific embodiments, the multi-arc ion plating method for preparing the NiCrAlYSi bonding layer specifically includes: placing the pretreated alloy sample on a sample table in a vacuum chamber, setting the distance between the sample and the target to about 260 mm, setting the sample holder rotation speed to 5 rpm, setting the vacuum chamber temperature to 500°C, and setting the vacuum degree in the furnace chamber to 4×10 -3 Pa, clean and activate the substrate surface. The coating preparation is divided into two stages: the first stage is to prepare the NiCrAlYSi base layer, and the second stage is to prepare the NiCrAlYSi coating. The reaction gas is nitrogen, the nitrogen flow rate is 30sccm, and the control pressure is 1Pa; the substrate bias is -80V, the arc current is 100A, and the deposition time is about 80-120min, and a bonding layer with a thickness of 30-60μm is obtained.

[0016] In some more specific embodiments, the preparation of the NiAlX bonding layer by electron beam physical vapor deposition specifically includes: placing the pretreated alloy substrate sample on a rotating base plate of an electron beam physical vapor deposition device, and then placing the target material rod to be evaporated into a water-cooled copper crucible, and evacuating the deposition chamber to 10 -3 ~10 -2 Pa, preheat the substrate to 800-900°C, adjust the electron beam voltage to 17-20 kV, the electron beam current to 1.0 A-1.2 A, the sample rotation rate to 10-12 rpm, the deposition time to 30-40 min, and obtain a bonding layer with a thickness of 30-60 μm.

[0017] In some more specific embodiments, the use of electroplating and embedding method to prepare the NiPtAl metal bonding layer specifically includes: selecting 20g / L diammine platinum nitrite (Pt(NH3)2(NO2)2), 120g / L ammonium nitrate (NH4NO3), 12g / L sodium nitrite (NaNO2) and 55g / L ammonia water (NH3·H2O) and placing them in a reactor and evenly mixing them into a Pt plating solution, and heating the Pt plating solution to 80°C, further placing the high-temperature alloy in the Pt plating solution, and setting the current to 0.8~1.0mA / mm 2 The electroplating time is 60 to 80 minutes, and a 4 to 5 μm electroplated Pt layer is prepared; the Pt layer is treated with aluminum by an embedding method, and the process parameters are: a holding temperature of 950 to 1000°C, a holding time of 90 to 120 minutes, and a 30 to 60 μm NiPtAl bonding layer is obtained.

[0018] The Al2O3-modified YSZ composite thermal barrier coating for preventing CMAS corrosion provided by the present invention has a dense structure, low thermal conductivity, and good high-temperature phase stability, and can effectively prevent the penetration of molten CMAS. Under conditions of high temperature above 1300°C and the presence of molten CMAS corrosion, the bottom of the AYSZ layer of the coating and the YSZ layer can still maintain structural integrity. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0020] Figure 1 A schematic diagram of the structure of an Al2O3-modified YSZ composite thermal barrier coating resistant to high-temperature CMAS corrosion provided by the present invention;

[0021] Figure 2 Schematic diagram of the structure of the homemade Al2O3-YSZ composite target. DETAILED DESCRIPTION

[0022] The solution provided in this specification is described below in conjunction with the accompanying drawings.

[0023] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be described below in conjunction with the accompanying drawings.

[0024] In the description of the embodiments of the present application, words such as "exemplary", "for example" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "exemplary", "for example" or "for example" in the embodiments of the present application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of words such as "exemplary", "for example" or "for example" is intended to present related concepts in a concrete way.

[0025] In the description of the embodiments of the present application, the term "and / or" is merely a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists alone, B exists alone, and A and B exist at the same time. In addition, unless otherwise specified, the term "plurality" means two or more.

[0026] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. The terms "include", "comprises", "has" and their variations all mean "including but not limited to", unless otherwise specifically emphasized.

[0027] The applicant found that the use of Al2O3 ceramic modification can cause CMAS to crystallize when it first contacts the coating surface, forming a dense high-melting point compound that hinders further penetration of the CMAS melt; at the same time, the high melting point characteristics of Al2O3 doping can also effectively prevent the YSZ coating from sintering prematurely, which plays a vital role in improving the high-temperature stability of the coating and extending its service life.

[0028] Based on this, the present invention designs an Al2O3-modified YSZ composite thermal barrier coating resistant to high temperature CMAS corrosion. The structural schematic diagram of the composite thermal barrier coating is as follows: Figure 1 As shown, the composite thermal barrier coating includes a metal bonding layer and a composite ceramic structural coating on a high-temperature alloy substrate, wherein the composite ceramic structural coating includes a first ceramic layer (YSZ layer) located on the inside and a second ceramic layer (Al2O3 modified YSZ (AYSZ) layer) located on the outside. After the composite thermal barrier coating coated with CMAS on the surface is heat treated at 1300°C for 50 hours, CMAS and the AYSZ layer form a 10-15μm sacrificial reaction layer, the main components of which are dense calcium feldspar phase and spinel phase formed by Al, Ca, Mg, and Si. The reaction layer can effectively prevent further penetration of CMAS, so that the bottom of the AYSZ layer and the YSZ layer maintain structural integrity under high temperature conditions above 1300°C.

[0029] In some embodiments, the first ceramic layer (YSZ layer) is deposited by electron beam evaporation of a YSZ target (8wt.% Y2O3-Zr2O) with a thickness of 100-125μm. The second ceramic layer (AYSZ layer) is made by electron beam bombardment of a self-made Al2O3-YSZ composite target (AYSZ target), with an Al2O3 content of 20wt.% to 30wt.% of the AYSZ composite coating, and the AYSZ layer thickness is 45-75μm. The total thickness of the composite ceramic structure coating does not exceed 200μm.

[0030] In some embodiments, the metal bonding layer includes one of the following three materials: the first is NiCrAlYSi, whose components include 40-60wt.% Ni, 14-28wt.% Cr, 15-20wt.% Al, 0.05-2wt.% Y and 0.05-2wt.% Si; the second is NiAlX, X is any one of Hf, Zr, Dy, and Y, and its components include 40-60wt.% Ni, 36-60wt.% Al, and 0.05-2wt.% X; the third is NiPtAl, whose components include 40-60mol.% Ni, 18-22mol.% Pt, and 30-45mol.% Al.

[0031] In some embodiments, the thickness of the metal bonding layer is 30-60 μm.

[0032] The above is a detailed introduction to the design concept and structural features of the composite thermal barrier coating of the present invention. Next, the preparation method of the composite thermal barrier coating provided by the present invention is specifically described. The specific steps of the method are as follows:

[0033] The first step is pretreatment of the high-temperature alloy substrate.

[0034] Prepare nickel-based high-temperature alloy, grind the surface of the alloy substrate with 80#, 200#, 600#, 800#, and 1000# sandpaper respectively, and polish it with Al2O3 slurry. After cleaning the alloy surface with ethanol, perform sandblasting pretreatment to control the surface roughness Ra of the alloy sample to 0.8μm and set it aside.

[0035] The second step is to prepare a metal bonding layer on the surface of the high-temperature alloy.

[0036] The metal bonding layer can be prepared by any of the following three methods: a) preparing NiCrAlYSi bonding layer by multi-arc ion plating method; b) preparing NiAlX bonding layer by electron beam physical vapor deposition, where X is any one of Hf, Zr, Dy, and Y; c) preparing NiPtAl metal bonding layer by electroplating and embedding method.

[0037] a) Preparation of NiCrAlYSi bonding layer by multi-arc ion plating method: The pretreated sample was placed on the sample stage of the vacuum chamber, the distance between the sample and the target was set to about 260 mm, the sample holder speed was 5 rpm, the vacuum chamber temperature was 500 °C, and the vacuum degree in the furnace during ion bombardment was 4 × 10 -3 Pa, clean and activate the substrate surface. The coating preparation is divided into two stages: the first stage is to prepare the NiCrAlYSi base layer, and the second stage is to prepare the NiCrAlYSi coating. The reaction gas is N2, the flow rate is 30sccm, and the control pressure is 1Pa. The substrate bias is -80V, the arc current is 100A, and the deposition time is about 80 to 120min, and a bonding layer with a thickness of 30 to 60μm is obtained.

[0038] b) Preparation of NiAlX bonding layer by electron beam physical vapor deposition: The pretreated alloy substrate sample was placed on the rotating base plate of the electron beam physical vapor deposition equipment, and then the target rod to be evaporated was placed in a water-cooled copper crucible, and the deposition chamber was evacuated to 10 -3 ~10 -2 Pa, preheat the substrate to 800-900°C, adjust the electron beam voltage to 17-20kV, the electron beam current to 1.0A-1.2A, and the sample rotation rate to 10-12rpm. The deposition time of the present invention is 30-40min, and a bonding layer with a thickness of 30-60μm is obtained.

[0039] c) Preparation of NiPtAl metal bonding layer by electroplating and embedding method: 20 g / L diammine platinum nitrite (Pt(NH3)2(NO2)2), 120 g / L ammonium nitrate (NH4NO3), 12 g / L sodium nitrite (NaNO2) and 55 g / L ammonia water (NH3·H2O) were placed in a reactor and evenly mixed to form a Pt plating solution, and the Pt plating solution was heated to 80°C, the high-temperature alloy was placed in the Pt plating solution, and the current was set to 0.8-1.0 mA / mm 2 The electroplating time is 60 to 80 minutes, and a 4 to 5 μm electroplated Pt layer is prepared; the Pt layer is treated with aluminum by an embedding method, and the process parameters are: a holding temperature of 950 to 1000°C, a holding time of 90 to 120 minutes, and finally a 30 to 60 μm NiPtAl is prepared as a metal bonding layer.

[0040] After the metal bonding layer is prepared, the high-temperature alloy is taken out and placed in a vacuum annealing furnace for vacuum heat treatment at a temperature of 1050-1150°C for 2-4 hours and a vacuum degree of 7-9×10 -5 mbar, cooled in the furnace and taken out at room temperature.

[0041] The third step is to prepare a composite ceramic structure coating on the surface of the metal bonding layer, and the steps are as follows:

[0042] The sample to be evaporated is placed on the electron beam physical vapor deposition rotating substrate, and the two target rods to be evaporated are placed in a water-cooled copper crucible. The vacuum degree of the deposition chamber is adjusted to 10 -3 Pa, substrate preheating 900-980°C, oxygen flux 100-105sccm, voltage 18-19kV, sample substrate rotation speed 15rpm. Prioritize the deposition of YSZ layer, switch the target to be evaporated to YSZ target, control the electron beam current to 0.65-0.76A, deposition time 35-45min, and obtain a 100-125μm YSZ layer; then deposit the AYSZ layer, switch the target to be evaporated to AYSZ target, adjust the electron beam current to 0.69-0.73A, deposition time 20-22min, and obtain a 45-75μm AYSZ layer.

[0043] The AYSZ target in the third step is a self-made Al2O3-YSZ composite target, and its structural diagram is shown in Figure 2 As shown. A hole with a diameter of 30 mm and a depth of 20 mm is dug at the bottom of a YSZ target material with a total thickness of 60 mm and a diameter of 68 mm, and an Al2O3 target material with the same inner diameter (30 mm) and thickness (~20 mm) is placed in the hole to obtain the Al2O3-YSZ composite target material. When the electron beam is evaporated, the composite target material is inverted, and the electron beam gun excitation is located at the junction of the YSZ target material and the Al2O3 target material. The distribution ratio of Al2O3 and YSZ components in the AYSZ coating is controlled by changing the position of the electron beam gun.

[0044] The composite thermal barrier coating and the preparation method thereof provided by the present invention are specifically introduced below in conjunction with the embodiments.

[0045] Example 1

[0046] The NiCrAlYSi bonding layer + electron beam physical vapor deposition composite ceramic structure coating is prepared by multi-arc ion plating on the surface of the high-temperature alloy. The specific steps are as follows:

[0047] The first step is to prepare a high temperature alloy test piece with a size of 20mm×3mm, polished with 80#, 200#, 600#, 800#, 1000# sandpaper respectively, polished with Al2O3, put into ethanol ultrasonic cleaning for 10 minutes, and then sandblasted, the surface roughness Ra of the test piece was controlled to 0.8μm, and set aside.

[0048] In the second step, a NiCrAlYSi bonding layer is prepared on the surface of the high-temperature alloy by a multi-arc ion plating method.

[0049] The pretreated sample was placed on the sample stage of the vacuum chamber. The distance between the sample and the target was set to about 260 mm. The sample holder speed was 5 rpm. The vacuum chamber temperature was 500 °C. The vacuum degree in the furnace during ion bombardment was 4 × 10-3 Pa, clean and activate the substrate surface. The coating preparation is divided into two stages: the first stage is to prepare the NiCrAlYSi base layer, and the second stage is to prepare the NiCrAlYSi coating. The reaction gas is nitrogen, the flow rate is 30sccm, and the control pressure is 1Pa. The substrate bias is -80V, the arc current is 100A, and the deposition time is about 80 to 120min, and a bonding layer with a thickness of 30 to 60μm is obtained.

[0050] After the metal bonding layer is prepared, the high-temperature alloy is taken out and placed in a vacuum annealing furnace for vacuum heat treatment at a temperature of 1050-1150°C for 2-4 hours and a vacuum degree of 7-9×10 -5 mbar, cooled in the furnace and taken out at room temperature.

[0051] The third step is to prepare a composite ceramic structure coating on the surface of the metal bonding layer, and the steps are as follows:

[0052] The sample to be evaporated is placed on the electron beam physical vapor deposition rotating substrate, and the two target rods to be evaporated are placed in a water-cooled copper crucible. The vacuum degree of the deposition chamber is adjusted to 10 -3 Pa, substrate preheating 900-980°C, oxygen flux 100-105sccm, voltage 18-19kV, sample substrate rotation speed 15rpm. Prioritize the deposition of YSZ layer, switch the target rod to YSZ target, control the electron beam current to 0.65-0.76A, deposition time 35-45min, and obtain a 100-125μm YSZ layer; then deposit the AYSZ layer, switch the target rod to AYSZ target, adjust the electron beam current to 0.69-0.73A, deposition time 20-22min, and obtain a 45-75μm AYSZ layer.

[0053] The prepared coating was observed by microscopic morphology and thickness. It can be found that the thickness of the NiCrAlYSi bonding layer is ~35μm, the thickness of the YSZ layer in the composite ceramic structure coating is ~105μm, and the thickness of the AYSZ layer is ~45μm. The composite ceramic structure coating has a columnar structure and the AYSZ layer is dense. CMAS was coated on the surface of the coating. After heat treatment at 1300℃ for 50h, a 10-15μm reaction sacrificial layer was formed on the surface of the AYSZ layer, and CMAS no longer invaded the bottom coating; the entire composite coating remained stable under high temperature and long-term conditions, and no obvious phase change occurred. The coating microstructure and columnar dendrites did not produce sintering phenomenon. The thermal conductivity of the composite coating at 1300℃ was measured to be about 1.65W / m·K, which is lower than that of the YSZ coating under the same temperature conditions, indicating that the coating maintains a good thermal insulation effect.

[0054] Example 2

[0055] The NiAlX bonding layer + composite ceramic structure coating was prepared by electron beam physical vapor deposition on the surface of the high-temperature alloy. The specific steps are as follows:

[0056] The first step is to prepare a high temperature alloy test piece with a size of 20mm×3mm, polished with 80#, 200#, 600#, 800#, 1000# sandpaper respectively, polished with Al2O3, put into ethanol ultrasonic cleaning for 10 minutes, and then sandblasted, the surface roughness Ra of the test piece was controlled to 0.8μm, and set aside.

[0057] In the second step, a NiPtAl bonding layer is prepared on the surface of the high-temperature alloy by electron beam physical vapor deposition.

[0058] High-purity nickel and high-purity aluminum (both nickel and aluminum have a purity greater than 99.99wt.%) and X (X is one of Hf, Zr, Dy, and Y) with a purity of 99.97wt.%, according to the composition design ratio: Al content is 50at.%, X content is 0.5at.%, and the balance is Ni. The surface of each alloy block is polished to remove the surface oxide scale, and then placed in anhydrous ethanol solution for ultrasonic cleaning for 20 minutes, and after drying, the prepared alloy is arc-melted to obtain 68.5×100mm metal layer target.

[0059] The target material was placed in a vacuum heat treatment furnace and heat treated at 1200° C. for 30 hours.

[0060] The pretreated alloy matrix sample was placed on the rotating base plate of the electron beam physical vapor deposition equipment, and then the NiAlX target to be evaporated was placed in a water-cooled copper crucible, and the deposition chamber was evacuated to 10 -3 ~10 -2 Pa, preheat the substrate to 800-900°C, adjust the electron beam voltage to 17-20 kV, the electron beam current to 1.0 A-1.2 A, and the sample rotation rate to 10-12 rpm. The deposition time is 35 min, and a bonding layer with a thickness of 40 μm is obtained.

[0061] After the metal bonding layer is prepared, the high-temperature alloy is taken out and placed in a vacuum annealing furnace for vacuum heat treatment at a temperature of 1150°C for 3 h and a vacuum degree of 7 to 9×10 -5 mbar, cooled in the furnace and taken out at room temperature.

[0062] The third step is to prepare a composite ceramic structure coating on the surface of the metal bonding layer, and the steps are as follows:

[0063] The sample to be evaporated is placed on the electron beam physical vapor deposition rotating substrate, and the two target rods to be evaporated are placed in a water-cooled copper crucible. The vacuum degree of the deposition chamber is adjusted to 10 -3Pa, substrate preheating 900-980°C, oxygen flux 100-105sccm, voltage 18-19kV, sample substrate rotation speed 15rpm. Prioritize the deposition of YSZ layer, switch the target rod to YSZ target, control the electron beam current to 0.65-0.76A, deposition time 35-45min, and obtain a 100-125μm YSZ layer; then deposit the AYSZ layer, switch the target rod to AYSZ target, adjust the electron beam current to 0.69-0.73A, deposition time 20-22min, and obtain a 45-75μm AYSZ layer.

[0064] The prepared coating was observed by microscopic morphology and thickness. It can be found that the thickness of the NiPtAl bonding layer is ~40μm, the thickness of the YSZ layer in the composite ceramic structure coating is ~100μm, and the thickness of the AYSZ layer is ~50μm. The composite ceramic structure coating has a columnar structure and the AYSZ layer is relatively dense. CMAS was coated on the surface of the coating. After heat treatment at 1300℃ for 50h, a 10-15μm reaction sacrificial layer was formed on the surface of the AYSZ layer, and CMAS no longer invaded the bottom coating; the entire composite coating remained stable under high temperature and long-term conditions, without obvious phase change, and the coating microstructure and columnar dendrites did not produce sintering phenomenon. The thermal conductivity of the composite structure coating at 1300℃ was measured to be about 1.66W / m·K, which is lower than that of the YSZ coating under the same temperature conditions, indicating that the coating maintains a good thermal insulation effect.

[0065] Example 3

[0066] The NiPtAl metal bonding layer + electron beam physical vapor deposition composite ceramic structure coating is prepared by electroplating and embedding on the surface of the high-temperature alloy. The specific steps are as follows:

[0067] The first step is to prepare a high temperature alloy test piece with a size of 20mm×3mm, polished with 80#, 200#, 600#, 800#, 1000# sandpaper respectively, polished with Al2O3, put into ethanol ultrasonic cleaning for 10 minutes, and then sandblasted, the surface roughness Ra of the test piece was controlled to 0.8μm, and set aside.

[0068] In the second step, a NiPtAl metal bonding layer is prepared on the surface of the high-temperature alloy by electroplating and embedding method.

[0069] 20 g / L of diammine platinum nitrite (Pt(NH3)2(NO2)2), 120 g / L of ammonium nitrate (NH4NO3), 12 g / L of sodium nitrite (NaNO2) and 55 g / L of ammonia water (NH3·H2O) were placed in a reactor and uniformly mixed to form a Pt plating solution, and the Pt plating solution was heated to 80°C. The high-temperature alloy was further placed in the Pt plating solution and the current was set to 0.8-1.0 mA / mm 2The electroplating time is 60 to 80 minutes, and a 4 to 5 μm electroplated Pt layer is prepared; the Pt layer is treated with aluminum by an embedding method, and the process parameters are: a holding temperature of 950 to 1000°C, a holding time of 90 to 120 minutes, and finally a 30 to 60 μm NiPtAl is prepared as a metal bonding layer.

[0070] After the NiPtAl bonding layer is prepared, the high-temperature alloy is taken out and placed in a vacuum annealing furnace for vacuum heat treatment at a temperature of 1150°C for 2 to 4 hours and a vacuum degree of 7 to 9×10 -5 mbar, cooled in the furnace and taken out at room temperature.

[0071] The third step is to prepare a composite ceramic structure coating on the surface of the metal bonding layer, and the steps are as follows:

[0072] The sample to be evaporated is placed on the electron beam physical vapor deposition rotating substrate, and the two target rods to be evaporated are placed in a water-cooled copper crucible. The vacuum degree of the deposition chamber is adjusted to 10 -3 Pa, substrate preheating 900-980°C, oxygen flux 100-105sccm, voltage 18-19kV, sample substrate rotation speed 15rpm. Prioritize the deposition of YSZ layer, switch the target rod to YSZ target, control the electron beam current to 0.65-0.76A, deposition time 35-45min, and obtain a 100-125μm YSZ layer; then deposit the AYSZ layer, switch the target rod to AYSZ target, adjust the electron beam current to 0.69-0.73A, deposition time 20-22min, and obtain a 45-75μm AYSZ layer.

[0073] The prepared coating was observed by microscopic morphology and thickness. It can be found that the thickness of the NiPtAl bonding layer is ~45μm, the thickness of the YSZ layer in the composite ceramic structure coating is ~100μm, and the thickness of the AYSZ layer is ~48μm. The composite ceramic structure coating has a columnar structure and the AYSZ layer is relatively dense. CMAS was coated on the surface of the coating. After heat treatment at 1300℃ for 50h, a 10-15μm reaction sacrificial layer was formed on the surface of the AYSZ layer, and CMAS no longer invaded the bottom coating; the entire composite coating remained stable under high temperature and long-term conditions, and no obvious phase change occurred. The coating microstructure and columnar dendrites did not produce sintering phenomenon. The thermal conductivity of the composite structure coating at 1300℃ was measured to be about 1.65W / m·K, which is lower than that of the YSZ coating under the same temperature conditions, indicating that the coating maintains a good thermal insulation effect.

[0074] In summary, compared with the prior art, the composite thermal barrier coating proposed in the present invention has the following beneficial effects:

[0075] 1. The ceramic layer (YSZ layer + AYSZ layer) is prepared by electron beam physical vapor deposition, with high deposition efficiency, precise control of coating thickness and composition, strong bonding between the coating and the metal bonding layer and the high-temperature alloy substrate, and the columnar structure of the coating is conducive to reducing strain tolerance and improving the service life of the coating;

[0076] 2. The present invention creatively uses Al2O3-doped modified YSZ as the second ceramic layer. On the one hand, Al2O3 reacts with CMAS to form a high-melting-point compound, which hinders the spreading and penetration of CMAS and has the effect of slowing down the corrosion of the internal coating by CMAS. On the other hand, for the coating prepared by electron beam physical deposition, due to the large inter-column gaps in its columnar crystal structure, it is easy to form a channel for CMAS to flow and penetrate, and the second ceramic layer AYSZ has a denser structure and CMAS flows more slowly, which further prevents the first ceramic layer YSZ from being corroded and damaged.

[0077] 3. The high melting point Al2O3 modification can also help improve the high temperature phase stability of the original YSZ, further improve the high temperature sintering resistance of YSZ, inhibit the growth of nano-grains on the coating surface, and thus ensure the long service life of the thermal barrier coating at high temperature.

[0078] 4. The present invention adopts an AYSZ / YSZ double-layer ceramic structure. On the one hand, it uses Al2O3 doping modification to reduce the thermal diffusion coefficient and thermal conductivity of the original coating system, thereby obtaining a better thermal insulation effect than a single-layer YSZ ceramic layer; on the other hand, it solves the problem of a large difference in thermal expansion coefficient between the high-temperature alloy substrate and the AYSZ ceramic layer, thereby reducing the difference in thermal expansion coefficient between layers, which helps to improve bonding strength and reduce the risk of coating peeling.

[0079] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made on the basis of the technical solution of the present invention should be included in the scope of protection of the present invention.

Claims

1. A kind of Al resistant to high temperature CMAS corrosion 2 O 3 Modified YSZ composite thermal barrier coating, It is characterized in that The invention comprises a metal bonding layer and a composite ceramic structural coating on a high temperature alloy substrate, wherein the composite ceramic structural coating comprises a first ceramic layer (YSZ layer) located on the inner side and a second ceramic layer (Al2O3 layer) located on the outer side. 2 O 3 Modified YSZ (AYSZ) layer).

2. The composite thermal barrier coating according to claim 1, It is characterized in that The first ceramic layer (YSZ layer) is made of a YSZ target (8 wt.% Y 2 O 3 -Zr 2 O) is deposited by electron beam evaporation with a thickness of 100 to 125 μm; the second ceramic layer (AYSZ layer) is obtained by self-made Al 2 O 3 -YSZ composite target is made by electron beam bombardment, Al 2 O 3 The content is 20wt.% to 30wt.% of the AYSZ composite coating, the thickness of the AYSZ layer is 45 to 75μm, and the total thickness of the composite ceramic structure coating does not exceed 200μm.

3. The composite thermal barrier coating according to claim 1, It is characterized in that The metal bonding layer includes one of the following three materials: the first is NiCrAlYSi, whose components include 40-60wt.% Ni, 14-28wt.% Cr, 15-20wt.% Al, 0.05-2wt.% Y and 0.05-2wt.% Si; the second is NiAlX, X is any one of Hf, Zr, Dy, and Y, and its components include 40-60wt.% Ni, 36-60wt.% Al, and 0.05-2wt.% X; the third is NiPtAl, whose components include 40-60mol.% Ni, 18-22mol.% Pt, and 30-45mol.% Al.

4. The composite thermal barrier coating according to claim 1, It is characterized in that The thickness of the metal bonding layer is 30-60 μm.

5. A kind of Al resistant to high temperature CMAS corrosion 2 O 3 Preparation method of modified YSZ composite thermal barrier coating, It is characterized in that The following steps are involved: The first step is the pretreatment of high temperature alloy; The second step is to prepare a metal bonding layer on the surface of the high-temperature alloy. After the metal bonding layer is prepared, the alloy is taken out and placed in a vacuum furnace. The heat treatment temperature is set to 1050-1150°C, the time is 2-4h, and the vacuum degree is set to 7-9×10 -5 mbar, cooled in the furnace and taken out at room temperature; In the third step, a ceramic coating is prepared on the surface of the metal bonding layer by electron beam physical vapor deposition. The preparation process includes: placing the sample to be evaporated on the electron beam physical vapor deposition rotating substrate, placing the target material to be evaporated in the electron beam physical deposition crucible, and setting the vacuum degree of the deposition chamber to 10 -3 Pa, the substrate is preheated to 900-980°C, the oxygen flux is set to 100-105sccm, the voltage is controlled to 18-19kV, the sample substrate rotation speed is controlled to be constant at 15rpm, and the target rotation speed is 0.8r / min; YSZ coating is preferentially deposited on the surface of the metal bonding layer, YSZ target is selected, the electron beam current is 0.65-0.76A, and the deposition time is 35-45min, and a YSZ layer of 100-125μm can be obtained; then AYSZ (Al 2 O 3 Modified YSZ) layer, choose Al 2 O 3 -YSZ composite target (AYSZ target), electron beam current is 0.69-0.73A, deposition time is 20-22min, and 45-75μm AYSZ layer is obtained.

6. The method for preparing the composite thermal barrier coating according to claim 5, It is characterized in that In the second step, the metal bonding layer is prepared by any of the following three methods: preparing a NiCrAlYSi bonding layer by multi-arc ion plating; preparing a NiAlX bonding layer by electron beam physical vapor deposition; and preparing a NiPtAl metal bonding layer by electroplating and embedding.

7. The preparation method according to claim 6, It is characterized in that The method for preparing the NiCrAlYSi bonding layer by multi-arc ion plating specifically includes: placing the pretreated alloy sample on the sample stage of the vacuum chamber, setting the distance between the sample and the target material to about 260 mm, setting the sample holder speed to 5 rpm, setting the vacuum chamber temperature to 500° C., and setting the vacuum degree in the furnace chamber to 4×10 -3 Pa, clean and activate the substrate surface; the reaction gas is nitrogen, the nitrogen flow rate is 30sccm, and the controlled pressure is 1Pa; the substrate bias is -80V, the arc current is 100A, the deposition time is about 80 to 120min, and a bonding layer with a thickness of 30 to 60μm is obtained.

8. The preparation method according to claim 6, It is characterized in that The method of preparing the NiAlX bonding layer by electron beam physical vapor deposition specifically includes: placing the pretreated alloy substrate sample on a rotating base plate of an electron beam physical vapor deposition device, then placing the target material rod to be evaporated into a water-cooled copper crucible, and evacuating the deposition chamber to 10 -3 ~10 -2 Pa, preheat the substrate to 800-900°C, adjust the electron beam voltage to 17-20 kV, the electron beam current to 1.0 A-1.2 A, the sample rotation rate to 10-12 rpm, the deposition time to 30-40 min, and obtain a bonding layer with a thickness of 30-60 μm.

9. The preparation method according to claim 6, It is characterized in that The method of preparing the NiPtAl metal bonding layer by electroplating and embedding method specifically includes: selecting 20g / L diammine platinum nitrite (Pt(NH 3 ) 2 (NO 2 ) 2 )、120g / L ammonium nitrate (NH 4 NO 3 )、12g / L sodium nitrite (NaNO 2 ) and 55 g / L ammonia water (NH 3 ·H 2 O) is placed in a reaction kettle and evenly mixed into a Pt plating solution, and the Pt plating solution is heated to 80°C, and the high-temperature alloy is further placed in the Pt plating solution, and the current is set to 0.8-1.0 mA / mm 2 The electroplating time is 60 to 80 minutes, and a 4 to 5 μm electroplated Pt layer is prepared; the Pt layer is treated with aluminum by an embedding method, and the process parameters are: a holding temperature of 950 to 1000°C, a holding time of 90 to 120 minutes, and a 30 to 60 μm NiPtAl bonding layer is obtained.

10. The preparation method according to claim 5, It is characterized in that In the third step, Al 2 O 3 -YSZ composite target is made by digging a certain size of columnar holes at the bottom of the columnar YSZ target, and then placing Al 2 O 3 The target is placed in the hole; when the electron beam evaporates, the composite target is turned upside down, and the electron beam gun excites the YSZ target and Al 2 O 3 At the interface between the target and the material, the Al content in the AYSZ coating can be controlled by changing the electron beam gun position. 2 O 3 And YSZ composition ratio.

Citation Information

Cited By

  • Method for synchronously improving CMAS corrosion resistance and thermal shock resistance of YSZ thermal barrier coating

    CN119956287A

  • Thermal barrier coating, preparation method and application

    CN121087488A