Thin film preparation method based on LPCVD furnace tube, related thin film and equipment

Silicon oxide-silicon nitride thin film stacks were prepared by combining dry oxygen method and chemical vapor deposition method in LPCVD furnace tubes, which solved the pollution problem during wafer transfer, improved the film quality and reduced the cost, and achieved efficient semiconductors Improved device performance.

CN118996378APending Publication Date: 2024-11-22ZHUHAI CHUANGFEIXIN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411103254.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the preparation of silicon oxide-silicon nitride thin film stacking, silicon wafers are prone to introduce contamination when they are transferred between different devices, resulting in the impact of film quality and semiconductor device performance.

Method used

The film preparation method based on LPCVD furnace tube is adopted to grow silicon oxide films by dry oxygen method and deposit silicon nitride films in the same furnace tube using chemical vapor deposition method, avoiding contamination during wafer transfer, simplifying the type of equipment and process.

Benefits of technology

The quality of the silicon oxide-silicon nitride film stack is improved, the preparation cost and time cost are reduced, and the equipment footprint is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996378A_ABST
    Figure CN118996378A_ABST
Patent Text Reader

Abstract

The invention discloses a thin film preparation method based on an LPCVD furnace tube, a related thin film and equipment, and can be applied to the field of thin film preparation. Then, introducing oxidant gas, and growing a first silicon oxide film on the surface of the silicon wafer by a dry oxygen method at a preset oxidation temperature; and finally, introducing silane and nitrogen, and depositing a silicon nitride thin film on one side, deviating from the silicon wafer, of the silicon oxide thin film by a chemical vapor deposition method to obtain a silicon oxide-silicon nitride thin film lamination. Therefore, pollution can be prevented from being introduced in the process of transferring the silicon wafer, on one hand, the quality of the silicon oxide-silicon nitride film lamination can be improved, and then the performance of a semiconductor device is improved; and on the other hand, the silicon wafer does not need to be cleaned between the growth of the silicon oxide thin film and the deposition of the silicon nitride thin film, so that the preparation cost of the thin film can be reduced. In addition, the number of machines needing to be used is small, the variety is single, the occupied area is small, and the production cost can be greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of thin film preparation, and in particular to a thin film preparation method based on LPCVD furnace tubes, related thin films and equipment. Background Art

[0002] With the development of semiconductor technology, silicon oxide-silicon nitride film stacks are widely used as gate dielectric layers, passivation layers, isolation layers and other structures of semiconductor devices due to their excellent electrical insulation properties and chemical stability.

[0003] At present, silicon oxide is usually grown on the surface of silicon wafers using one machine, and then silicon nitride is deposited on the surface of silicon oxide using another machine to prepare silicon oxide-silicon nitride film stacks. However, in the process of transferring silicon wafers from one machine to another, contamination is easily introduced, resulting in a high degree of defects in the deposited silicon nitride film, which affects the quality of the film and the performance of semiconductor devices.

[0004] Therefore, how to obtain high-quality silicon oxide-silicon nitride thin film stacks becomes a problem that needs to be solved. Summary of the invention

[0005] Based on the above problems, the present application provides a thin film preparation method, related films and equipment based on LPCVD furnace tubes, which can prepare high-quality silicon oxide-silicon nitride thin film stacks.

[0006] The embodiments of the present application disclose the following technical solutions:

[0007] In a first aspect, an embodiment of the present application provides a method for preparing a thin film based on a LPCVD furnace tube, the method comprising:

[0008] Provide silicon wafers;

[0009] introducing an oxidant gas, and growing a first silicon oxide film on the surface of the silicon wafer by a dry oxygen method at a preset oxidation temperature;

[0010] Silane and nitrogen are introduced to deposit a silicon nitride film on the side of the silicon oxide film away from the silicon wafer by chemical vapor deposition to obtain a silicon oxide-silicon nitride film stack.

[0011] Optionally, the step of introducing silane and nitrogen to deposit a silicon nitride film on a side of the silicon oxide film away from the silicon wafer by chemical vapor deposition to obtain a silicon oxide-silicon nitride film stack comprises:

[0012] Silane, dichlorosilane and nitrogen are introduced to deposit a silicon nitride film by chemical vapor deposition to obtain a silicon oxide-silicon nitride film stack.

[0013] Optionally, the preset oxidation temperature is selected from between 700°C and 1200°C.

[0014] Optionally, after the silicon oxide-silicon nitride film stack is obtained by introducing silane and nitrogen to deposit a silicon nitride film on the side of the silicon oxide film away from the silicon wafer by chemical vapor deposition to obtain the silicon oxide-silicon nitride film stack, the method further comprises:

[0015] Inert gas and cleaning gas are introduced in sequence to remove pollutants on the surface of the silicon nitride film.

[0016] Optionally, after the silane and nitrogen are introduced and a silicon nitride film is deposited on a side of the silicon oxide film away from the silicon wafer by chemical vapor deposition to obtain a silicon oxide-silicon nitride film stack, the method further comprises:

[0017] An oxidant gas is introduced, and at a preset oxidation temperature, a second silicon oxide film is grown on the side of the silicon nitride film away from the silicon wafer by a dry oxygen method to obtain a silicon oxide-silicon nitride-silicon oxide film stack.

[0018] Optionally, after the silane and nitrogen are introduced and a silicon nitride film is deposited on a side of the silicon oxide film away from the silicon wafer by chemical vapor deposition to obtain a silicon oxide-silicon nitride film stack, the method further comprises:

[0019] An oxidant gas and a silicon source are introduced, and a second silicon oxide film is deposited on the side of the silicon nitride film away from the silicon wafer by chemical vapor deposition to obtain a silicon oxide-silicon nitride-silicon oxide film stack.

[0020] Optionally, before providing the silicon wafer, the method further includes:

[0021] Monitor the vacuum degree in the furnace tube;

[0022] If the vacuum degree meets the preset conditions, then: the temperature in the furnace tube is increased until the temperature in the furnace tube reaches the preset cleaning temperature; nitrogen is introduced until the pressure in the furnace tube reaches the preset pressure;

[0023] Introduce inorganic non-metallic fluoride gas to clean the furnace tube.

[0024] In a second aspect, an embodiment of the present application provides a silicon oxide-silicon nitride thin film stack, wherein the silicon oxide-silicon nitride thin film stack is prepared by the thin film preparation method based on the LPCVD furnace tube described in any embodiment of the first aspect.

[0025] In a third aspect, an embodiment of the present application provides a silicon oxide-silicon nitride-silicon oxide thin film stack, and the silicon oxide-silicon nitride-silicon oxide thin film stack is prepared by the thin film preparation method based on the LPCVD furnace tube described in the corresponding embodiment of the first aspect.

[0026] In a fourth aspect, an embodiment of the present application provides a LPCVD furnace tube, which is used to execute the thin film preparation method based on the LPCVD furnace tube described in any embodiment of the first aspect.

[0027] Compared with the prior art, this application has the following beneficial effects:

[0028] The embodiment of the present application provides a thin film preparation method based on an LPCVD furnace tube, in which, first, a silicon wafer is provided; then, an oxidant gas is introduced, and a first silicon oxide film is grown on the surface of the silicon wafer by a dry oxygen method at a preset oxidation temperature; finally, silane and nitrogen are introduced, and a silicon nitride film is deposited on the side of the silicon oxide film away from the silicon wafer by a chemical vapor deposition method to obtain a silicon oxide-silicon nitride film stack. Thus, in the same LPCVD furnace tube, the first silicon oxide film is grown by a dry oxygen method and the silicon nitride film is deposited by a chemical vapor deposition method, and there is no need to transfer the silicon wafer between the two machines in the middle, which can save the time cost of preparing the silicon oxide-silicon nitride film stack and avoid the introduction of pollution in the process of transferring the silicon wafer. On the one hand, the quality of the silicon oxide-silicon nitride film stack can be improved, thereby improving the performance of the semiconductor device; on the other hand, there is no need to clean the silicon wafer between growing the silicon oxide film and depositing the silicon nitride film, which can reduce the preparation cost of the film. In addition, the preparation of silicon oxide-silicon nitride thin film stacks can be achieved using only one LPCVD furnace tube. The number of machines required is small and the type is single, which occupies a small area and can greatly reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 A flow chart of a thin film preparation method based on LPCVD furnace tube provided in an embodiment of the present application;

[0031] Figure 2 A flow chart of another thin film preparation method based on LPCVD furnace tube provided in an embodiment of the present application;

[0032] Figure 3 A schematic diagram of a thin film structure in a process of preparing a thin film based on an LPCVD furnace tube provided in an embodiment of the present application. DETAILED DESCRIPTION

[0033] The thin film preparation method based on LPCVD furnace tubes, related thin films and equipment provided in the present application can be used in the field of thin film preparation. The above is only an example and does not limit the application field of the thin film preparation method based on LPCVD furnace tubes, related thin films and equipment provided in the present application.

[0034] The terms "first", "second", "third" and "fourth" etc. in the specification, claims and drawings of this application are used to distinguish different objects rather than to limit a specific order.

[0035] In the embodiments of the present application, the words "as an example" or "for example" are used to indicate examples, illustrations or explanations. Any embodiment or design described as "as an example" or "for example" in the embodiments of the present application should not be interpreted as being more preferred or more advantageous than other embodiments or designs. Specifically, the use of the words "as an example" or "for example" is intended to present the relevant concepts in a specific way.

[0036] The terms used in the implementation section of this application are only used to explain the specific embodiments of this application and are not intended to limit this application.

[0037] Chemical Vapor Deposition (CVD) technology has the advantages of low deposition temperature, easy control of film composition and thickness, good uniformity and repeatability, simple operation and wide range of applications. It has gradually become the mainstream method for preparing thin films in the semiconductor field.

[0038] Low Pressure Chemical Vapor Deposition (LPCVD) is a type of CVD technology that allows precursor gases to react at a relatively low pressure, thereby depositing a reactant film on a substrate. During the operation of the LPCVD furnace tube, the internal pressure of the furnace tube is usually in the range of 1 torr to 100 torr.

[0039] The inventors found that although the thin film produced by the LPCVD method has advantages in uniformity and repeatability, the silicon oxide layer deposited by the LPCVD method has poor density; while dry oxidation can usually produce a silicon oxide layer with higher density.

[0040] At present, the stacking of high-density silicon oxide layer and silicon nitride layer is increasingly used in semiconductor devices. In order to obtain a film that meets the requirements, it is usually necessary to first dry-oxidize the silicon wafer in an oxidation furnace to prepare the silicon oxide layer; then, the silicon wafer is transferred to the LPCVD furnace tube for the deposition of the nitride layer. However, in the process of transferring the silicon wafer from one machine to another, contamination is easily introduced, resulting in a high degree of defects in the deposited silicon nitride film, which affects the quality of the film and the performance of the semiconductor device.

[0041] In view of this, the embodiment of the present application provides a thin film preparation method based on an LPCVD furnace tube, in which, first, a silicon wafer is provided; then, an oxidant gas is introduced, and a first silicon oxide film is grown on the surface of the silicon wafer by a dry oxygen method at a preset oxidation temperature; finally, silane and nitrogen are introduced, and a silicon nitride film is deposited on the side of the silicon oxide film away from the silicon wafer by a chemical vapor deposition method to obtain a silicon oxide-silicon nitride film stack. Thus, in the same LPCVD furnace tube, the first silicon oxide film is grown by a dry oxygen method and the silicon nitride film is deposited by a chemical vapor deposition method, and there is no need to transfer the silicon wafer between the two machines in the middle, which can save the time cost of preparing the silicon oxide-silicon nitride film stack and avoid the introduction of pollution in the process of transferring the silicon wafer. On the one hand, the quality of the silicon oxide-silicon nitride film stack can be improved, thereby improving the performance of the semiconductor device; on the other hand, there is no need to clean the silicon wafer between growing the silicon oxide film and depositing the silicon nitride film, which can reduce the preparation cost of the film. In addition, the preparation of silicon oxide-silicon nitride thin film stacks can be achieved using only one LPCVD furnace tube. The number of machines required is small and the type is single, which occupies a small area and can greatly reduce production costs.

[0042] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0043] See also Figure 1 , which is a flow chart of a thin film preparation method based on LPCVD furnace tube provided by the present application, the method comprising:

[0044] S101: Provide silicon wafers.

[0045] As an example, silicon wafers can be placed on a wafer boat and transferred to a LPCVD furnace tube via the wafer boat.

[0046] Optionally, before the silicon wafer is transferred to the LPCVD furnace tube, it can be pre-cleaned by methods such as chemical cleaning, plasma cleaning or ultrasonic cleaning to remove particles and contaminants on the surface of the silicon wafer, so as to facilitate the preparation of high-quality thin films on the surface of the silicon wafer.

[0047] Optionally, in this embodiment, the LPCVD furnace tube can be used to prepare silicon oxide by dry oxidation method and to deposit silicon nitride by chemical vapor deposition method. Since the oxidation reaction itself does not produce particles in the dry oxidation process, but more particles are produced in the chemical vapor deposition process, multiple wafer boats can be prepared for the process requiring chemical vapor deposition and the process only performing dry oxidation, respectively, to avoid mixing the wafer boat for chemical vapor deposition with the wafer boat for dry oxidation method, resulting in the residual particles on the wafer boat affecting the quality of silicon oxide obtained by dry oxidation method.

[0048] S102: introducing an oxidant gas, and growing a first silicon oxide film on the surface of the silicon wafer by a dry oxygen method at a preset oxidation temperature.

[0049] Optionally, after placing the wafer boat containing the silicon wafers in the furnace tube, the furnace door of the furnace tube can be closed and evacuated to exhaust the gas in the furnace tube; then the temperature in the furnace tube is heated to a preset oxidation temperature; then, an inert gas such as nitrogen can be introduced to further remove the residual gas in the furnace tube after evacuation and establish a stable atmosphere environment; after the temperature in the furnace tube is stabilized, an oxidant gas such as oxygen can be introduced.

[0050] The preset oxidation temperature may be selected from 700° C. to 1200° C.; in another embodiment, the preset oxidation temperature may also be selected from 900° C. to 1100° C.; the oxidation temperature may be set based on factors such as the required silicon oxide thickness.

[0051] At a preset oxidation temperature, the oxidant gas can pass through the silicon oxide layer formed on the surface of the silicon wafer, and continuously react chemically with the silicon atoms on the surface of the silicon wafer, so that the thickness of the formed silicon oxide layer gradually increases, thereby growing a first silicon oxide film with high density on the surface of the silicon wafer by dry oxygen method in the absence of water vapor. The thickness of the grown first silicon oxide film can be controlled by controlling the oxidation temperature and oxidation time, and the thickness of the first silicon oxide film can be selected from For example, it can be

[0052] Optionally, the growth of the first silicon oxide film may be performed under low pressure conditions, thereby improving the uniformity and quality of the first silicon oxide film.

[0053] S103: introducing silane and nitrogen to deposit a silicon nitride film on the side of the silicon oxide film facing away from the silicon wafer by chemical vapor deposition to obtain a silicon oxide-silicon nitride film stack.

[0054] Optionally, after growing the first silicon oxide film, the introduction of the oxidant gas is stopped first; then, an inert gas such as nitrogen is used for flushing to remove the residual oxidant gas in the furnace tube to avoid the oxidant gas mixing with the subsequently introduced silane and causing safety accidents. For example, a mixture of oxygen and silane may burn or even explode; then, the concentration of the residual gas in the furnace tube can be further reduced by vacuuming to reduce the risk of the residual oxidant gas reacting with silane; after vacuuming, silane and nitrogen are introduced into the furnace tube again.

[0055] Specifically, silane (SiH4) provides a silicon source, and nitrogen (N2) provides a nitrogen source, and the two react chemically, and the reaction equation can be simplified to: 3SiH4+4N2→Si3N4+12H2. Thus, silane reacts with nitrogen to generate silicon nitride (Si3N4) particles, which are deposited on the side of the silicon oxide film away from the silicon wafer to form a silicon nitride film, thereby forming a silicon oxide-silicon nitride film stack.

[0056] In the embodiment of the present application, in the same LPCVD furnace tube, the first silicon oxide film is grown by dry oxygen method and the silicon nitride film is deposited by chemical vapor deposition method, and there is no need to transfer the silicon wafer between the two machines in the middle, which can save the time cost of preparing the silicon oxide-silicon nitride film stack and avoid the introduction of pollution in the process of transferring the silicon wafer. On the one hand, the quality of the silicon oxide-silicon nitride film stack can be improved, thereby improving the performance of semiconductor devices; on the other hand, there is no need to clean the silicon wafer between growing the silicon oxide film and depositing the silicon nitride film, which can reduce the preparation cost of the film. In addition, the preparation of the silicon oxide-silicon nitride film stack can be achieved using only one LPCVD furnace tube, the number of machines required is small and the type is single, the floor space is small, and the production cost can be greatly reduced.

[0057] See also Figure 2 , which is a flow chart of another thin film preparation method based on LPCVD furnace tube provided in an embodiment of the present application, the method comprising:

[0058] S201: Provide a silicon wafer.

[0059] S202: introducing an oxidant gas, and growing a first silicon oxide film on the surface of the silicon wafer by a dry oxygen method at a preset oxidation temperature.

[0060] Specifically, Figure 3 In (A), the oxidant chemically reacts with the surface of the silicon wafer at high temperature to form a first silicon oxide film.

[0061] S203: introducing silane, dichlorosilane and nitrogen to deposit a silicon nitride film by chemical vapor deposition to obtain a silicon oxide-silicon nitride film stack.

[0062] Specifically, silane (SiH4) and dichlorosilane (SiH2Cl2) provide silicon sources, and nitrogen (N2) provides nitrogen sources. Using low-pressure chemical vapor deposition, silane and nitrogen can undergo a chemical reaction: 3SiH4+4N2→Si3N4+6NH3; dichlorosilane and ammonia can undergo a chemical reaction: 3SiH2Cl2+4NH3→Si3N4+6HCl+6H2; silane and ammonia can undergo a chemical reaction: SiH4+2NH3→Si3N4+3H2.

[0063] Therefore, if Figure 3 In (B), silane, dichlorosilane and nitrogen are introduced into the LPCVD furnace tube, which can react more quickly to generate silicon nitride (Si3N4) particles. The silicon nitride particles are deposited on the side of the silicon oxide film away from the silicon wafer to form a silicon nitride film, which can increase the deposition rate of silicon nitride and help form a dense and uniform silicon nitride film, thereby forming a high-quality silicon oxide-silicon nitride film stack. The thickness of the silicon nitride film can be selected from For example, it can be

[0064] S204: Inert gas and cleaning gas are introduced sequentially to remove pollutants on the surface of the silicon nitride film.

[0065] As an example, after forming the silicon oxide-silicon nitride film stack, the introduction of gases such as silane can be stopped first; then, an inert gas such as nitrogen can be used for flushing to remove residual gases such as silane in the furnace tube to avoid safety accidents caused by the mixing of silane with the subsequently introduced oxidant gas; then, a cleaning gas such as oxygen, chlorine or halogen gas can be introduced to remove pollutants that may exist on the surface of the silicon nitride film, such as carbon deposits, silicon nitride particles and / or metal impurities, so as to improve the quality of the subsequently grown silicon oxide; then, the concentration of the residual gas in the furnace tube can be further reduced by vacuuming to reduce the adverse effects of the residual gas on the quality of the grown silicon oxide; after vacuuming, oxygen and nitrogen are introduced into the furnace tube for dry oxidation.

[0066] S205: introducing an oxidant gas, and growing a second silicon oxide film on the side of the silicon nitride film away from the silicon wafer by a dry oxygen method at a preset oxidation temperature to obtain a stack of silicon oxide-silicon nitride-silicon oxide.

[0067] Specifically, Figure 3In step (C), an oxidant gas, such as oxygen, is introduced to dry-oxidize the silicon wafer on which the silicon oxide-silicon nitride film stack is formed. The oxidant gas reacts with the silicon nitride to grow a second silicon oxide film on the side of the silicon nitride film away from the silicon wafer, thereby obtaining a silicon oxide-silicon nitride-silicon oxide film stack (i.e., an ONO layer) which is often used as a gate dielectric layer in a SONOS (Silicon-Oxide-Nitride-Oxide-Silicon) device. For example, the thickness of the second silicon oxide film can be

[0068] Optionally, after executing step S204, an oxidant gas and a silicon source may be introduced to deposit a second silicon oxide film on the side of the silicon nitride film facing away from the silicon wafer by chemical deposition, thereby obtaining a silicon oxide-silicon nitride-silicon oxide film stack.

[0069] As a result, a silicon oxide-silicon nitride-silicon oxide thin film stack can be prepared at one time in a LPCVD furnace tube, greatly reducing the equipment cost and time cost required for thin film preparation.

[0070] In another embodiment, before executing step S201 or after executing step S205 and taking out the wafer, the LPCVD furnace tube may be cleaned. The specific steps are as follows:

[0071] S1: Monitor the vacuum degree in the furnace tube.

[0072] Specifically, after the wafer is taken out, the furnace door of the furnace tube can be closed and vacuum can be drawn, and the vacuum degree in the furnace tube can be monitored to determine whether the subsequent cleaning steps can be started, thereby ensuring that the entire cleaning process is carried out in a controlled environment.

[0073] S2: If the vacuum degree in the furnace tube meets the preset conditions, then: the temperature in the furnace tube is increased until the temperature in the furnace tube reaches the preset cleaning temperature; nitrogen is introduced until the pressure in the furnace tube reaches the preset pressure.

[0074] Specifically, nitrogen may be introduced while the furnace tube is heated, or the temperature may be increased first and then the nitrogen may be introduced, or nitrogen may be introduced first and then the temperature is increased, which is not limited in the present embodiment.

[0075] Optionally, the preset cleaning temperature may be selected from 350° C. to 700° C., for example, 600° C. After the temperature is stabilized at the cleaning temperature, the introduction of nitrogen may be stopped.

[0076] Optionally, the preset pressure may be selected from 100 mtorr to 1000 mtorr, for example, 500 mtorr; during the cleaning process, the pressure in the furnace tube may be controlled to be within the range of 100 mtorr to 1000 mtorr.

[0077] S3: Introduce inorganic non-metallic fluoride gas to clean the furnace tube.

[0078] The inorganic non-metallic fluoride gas can react with the deposits on the inner wall of the furnace tube, thereby achieving the purpose of cleaning the furnace tube and reducing the impact of these deposits on the quality of the subsequently prepared thin film.

[0079] Optionally, after cleaning the furnace tube, the introduction of inorganic non-metallic fluoride gas can be stopped and nitrogen can be introduced again, which can not only drive away the incompletely reacted inorganic non-metallic fluoride gas and reaction products and provide back pressure, but also clean the furnace tube; after the pressure in the furnace tube approaches atmospheric pressure, the furnace door is unlocked to complete the cleaning.

[0080] Optionally, while back-pressuring, the temperature inside the furnace tube can also be lowered, wherein the cooling process can be: first lowering the temperature to 475°C, continuing for 2 minutes, then lowering the temperature again to 200°C, and continuing for another 2 minutes before lowering the temperature to room temperature. In this way, the remaining gas or reaction by-products of the complete reaction in the furnace tube can be reduced, and the thermal shock inside the furnace tube can be reduced, which helps to extend the service life of the furnace tube and prevent the furnace tube from being damaged due to uneven thermal expansion.

[0081] Therefore, the furnace tube can be cleaned before the silicon wafer to be subjected to the thin film preparation process is placed, thereby reducing the influence of the deposits in the furnace tube on the quality of the oxide layer grown by the dry oxygen method.

[0082] The present application also provides a silicon oxide-silicon nitride thin film stack, which is prepared by the above-mentioned LPCVD furnace tube-based thin film preparation method.

[0083] The present application also provides a silicon oxide-silicon nitride-silicon oxide thin film stack, which is prepared by the above-mentioned thin film preparation method based on the LPCVD furnace tube.

[0084] The present application also provides a LPCVD furnace tube for executing the thin film preparation method based on the LPCVD furnace tube described in any of the above embodiments.

[0085] It should be noted that the various embodiments in this specification are described in a progressive manner, and the same and similar parts between the various embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the device embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment. Ordinary technicians in this field can understand and implement it without paying creative work.

[0086] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a thin film based on a LPCVD furnace tube, characterized in that: The method comprises: Provide silicon wafers; introducing an oxidant gas, and growing a first silicon oxide film on the surface of the silicon wafer by a dry oxygen method at a preset oxidation temperature; Silane and nitrogen are introduced to deposit a silicon nitride film on the side of the silicon oxide film away from the silicon wafer by chemical vapor deposition to obtain a silicon oxide-silicon nitride film stack.

2. The method according to claim 1, characterized in that: The step of introducing silane and nitrogen to deposit a silicon nitride film on the side of the silicon oxide film away from the silicon wafer by chemical vapor deposition to obtain a silicon oxide-silicon nitride film stack comprises: Silane, dichlorosilane and nitrogen are introduced to deposit a silicon nitride film by chemical vapor deposition to obtain a silicon oxide-silicon nitride film stack.

3. The method according to claim 1, characterized in that The preset oxidation temperature is selected from 700°C to 1200°C.

4. The method according to claim 1, characterized in that: After the silane and nitrogen are introduced to deposit a silicon nitride film on the side of the silicon oxide film away from the silicon wafer by chemical vapor deposition to obtain a silicon oxide-silicon nitride film stack, the method further comprises: Inert gas and cleaning gas are introduced in sequence to remove pollutants on the surface of the silicon nitride film.

5. The method according to claim 1, characterized in that After introducing silane and nitrogen, depositing a silicon nitride film by chemical vapor deposition on the side of the silicon oxide film away from the silicon wafer to obtain a silicon oxide-silicon nitride film stack, the method further comprises: An oxidant gas is introduced, and at a preset oxidation temperature, a second silicon oxide film is grown on the side of the silicon nitride film away from the silicon wafer by a dry oxygen method to obtain a silicon oxide-silicon nitride-silicon oxide film stack.

6. The method according to claim 1, characterized in that After introducing silane and nitrogen, depositing a silicon nitride film by chemical vapor deposition on the side of the silicon oxide film away from the silicon wafer to obtain a silicon oxide-silicon nitride film stack, the method further comprises: An oxidant gas and a silicon source are introduced, and a second silicon oxide film is deposited on the side of the silicon nitride film away from the silicon wafer by chemical vapor deposition to obtain a silicon oxide-silicon nitride-silicon oxide film stack.

7. The method according to claim 1, characterized in that Before providing the silicon wafer, the method further includes: Monitor the vacuum degree in the furnace tube; If the vacuum degree meets the preset conditions, then: the temperature in the furnace tube is increased until the temperature in the furnace tube reaches the preset cleaning temperature; nitrogen is introduced until the pressure in the furnace tube reaches the preset pressure; Introduce inorganic non-metallic fluoride gas to clean the furnace tube.

8. A silicon oxide-silicon nitride thin film stack, characterized in that: The silicon oxide-silicon nitride thin film stack is prepared by the thin film preparation method based on the LPCVD furnace tube according to any one of claims 1 to 7.

9. A silicon oxide-silicon nitride-silicon oxide thin film stack, characterized in that: The silicon oxide-silicon nitride-silicon oxide thin film stack is prepared by the thin film preparation method based on the LPCVD furnace tube according to claim 5 or 6.

10. A LPCVD furnace tube, characterized in that: The furnace tube is used to execute the thin film preparation method based on the LPCVD furnace tube according to any one of claims 1 to 7.