Vanadium-doped nickel phosphide electrocatalyst and preparation method thereof

By doping vanadium elements in Ni2P catalyst, a three-dimensional nanoflower-shaped vanadium-doped nickel phosphide electrocatalyst was prepared, which solved the problems of high catalyst cost and high energy consumption in electrolytic hydrogen production technology, and achieved low cost and high cost Efficient hydrogen production significantly improves the performance of alkaline electrolytic hydrogen evolution reaction.

CN118996496AInactive Publication Date: 2024-11-22BEIJING UNIV OF CHEM TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310549963.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing electrolytic hydrogen production technology, the catalyst costs are high and the energy consumption is too high. Especially in alkaline systems, the catalyst performance is not ideal, making it difficult to achieve low-cost and high-efficiency hydrogen production.

Method used

Using Ni2P as the basic material, vanadium-doped nickel phosphide electrocatalyst is prepared by doping vanadium-like hydrothermal method and phosphating calcination method to catalyze the hydrogen evolution reaction of alkaline electrolytic water to improve the activity of the catalyst and stability.

Benefits of technology

A low-cost, high-activity and stable electrocatalyst is achieved, which significantly reduces the energy consumption of hydrogen production by electrolyzing water, improves hydrogen generation efficiency, and vanadium-doped vanadium-doped nickel phosphide catalysts exhibit excellent performance in alkaline media electrochemical hydrogen evolution properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996496A_ABST
    Figure CN118996496A_ABST
Patent Text Reader

Abstract

The invention relates to a vanadium-doped nickel phosphide electrocatalyst and a preparation method thereof, and belongs to the technical field of water electrolysis hydrogen production catalysts, the catalyst material is composed of a vanadium element, a nickel element and a phosphorus element and presents a Ni2P phase, the vanadium element is used as a doping element and does not form a phase independently, the material is in a three-dimensional nanoflower shape, the diameter distribution is 3-7 microns, and the diameter distribution is 3-7 microns. According to the specific preparation process of the material, ammonium metavanadate serves as a vanadium source, a nano-flower-shaped precursor is synthesized through a hydrothermal method, then the nano-flower-shaped vanadium-doped nickel phosphide material is synthesized after phosphating roasting, the synthesis method is simple and high in controllability, and the electrocatalytic hydrogen evolution material prepared through the method is excellent in electrochemical performance and suitable for industrial production. Vanadium doping can reduce the d-band center and adjust the electronic structure of nickel phosphide, and shows excellent hydrogen production catalytic activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a vanadium-doped nickel phosphide electrocatalyst and a preparation method thereof, belonging to the technical field of preparation of water electrolysis hydrogen evolution materials. Background Art

[0002] Hydrogen energy is considered to be one of the important candidate energy sources to replace fossil fuels and is hailed as the "ultimate energy" of the 21st century. Hydrogen production by water electrolysis (HER) is one of the current methods for producing green hydrogen. It has the advantages of simple process, no pollution, and high hydrogen purity, and is one of the most promising hydrogen production technologies. Since the oxygen evolution reaction is more likely to occur in alkaline systems, and compared with acidic electrolytes, alkaline electrolytes are less corrosive to catalysts and have a wider range of catalyst selection, alkaline water electrolysis is more suitable for commercial hydrogen production. However, since the hydrogen evolution reaction in the alkaline system requires the activation and decomposition of water first, the catalyst with high catalytic activity in the acidic system usually does not have ideal alkaline hydrogen evolution performance. Therefore, the biggest problem with hydrogen production by water electrolysis is that the energy consumption of the reaction process is too high, and catalysts need to be added to reduce the reaction energy barrier. At present, the best material for catalytic hydrogen production is still the expensive and limited precious metal platinum-based catalyst. Therefore, the key to efficient hydrogen production by water electrolysis lies in the development of low-cost and high-efficiency electrocatalysts.

[0003] Among the reported catalysts, transition metal phosphides (TMPs) are considered to be very promising HER electrocatalysts due to their low cost, good conductivity and high electrochemical stability. However, for alkaline HER, there is still a certain gap between the performance of TMPs and platinum-based catalysts. Therefore, the development of low-cost, highly active and stable TMPs is still worth exploring. The hydrogen evolution reaction in alkaline media involves the dissociation of water to form adsorbed *H and OH - According to the hydrogen binding energy theory, in alkaline HER, the adsorption and desorption of hydrogen atoms on the catalyst surface are two opposite processes. If the adsorption force is quite weak, it is not conducive to the production of hydrogen. On the contrary, if the adsorption force is quite strong, it is conducive to the production of hydrogen, but not conducive to the release of hydrogen. Therefore, there must be a balance between adsorption and desorption on the catalyst surface. The catalytic activity is usually expressed in terms of hydrogen adsorption free energy (ΔG H* ) is used to measure the ΔG of a good catalyst. H* It should be close to zero. Adjusting the electronic structure of the catalyst by doping is an effective way to adjust the adsorption energy of the reaction intermediates.

[0004] In the literature (1) Nanoscale, 2019, 11, 4198, Xinyang Li et al. used hydrothermal and calcination methods to in situ grow V-Ni2P / CC nanosheet arrays on carbon cloth. The multi-level structure increased the specific surface area of ​​the material. In the literature (2) ACS Appl. Nano Mater. 2021, 4, 10791-10798, Xiang Wu et al. used hydrothermal and calcination methods to prepare V-NiCoP / NF nanowire arrays on nickel foam. The nanowire arrays are conducive to the precipitation of H2. The above work has a significant effect in improving the charge transfer rate, but there is still a certain gap from practical application. In addition, the use of VCl3 as a vanadium source has a high preparation cost, which is not conducive to large-scale preparation. Therefore, the low-cost method to prepare hydrogen evolution electrocatalysts with excellent performance is still a very challenging and innovative task.

[0005] Based on this, in the present invention, Ni2P is used as the basic material, and vanadium is doped to modify it, and a powder nano-flower-shaped vanadium-doped Ni2P electrocatalyst is prepared for catalyzing the hydrogen evolution reaction in alkaline water electrolysis. Summary of the invention

[0006] The object of the present invention is to provide a vanadium-doped nickel phosphide electrocatalyst material, characterized in that the catalyst material is composed of vanadium, nickel and phosphorus, presenting a Ni2P phase, the vanadium element as a doping element does not form a separate phase, the molar ratio of vanadium to nickel is 0.03-0.08, the molar ratio of nickel to phosphorus is 2:1, and the material is a three-dimensional nanoflower with a diameter distribution of 3-7μm.

[0007] The present invention also provides a method of using ammonium metavanadate as a vanadium source, synthesizing a nano-flower-shaped precursor by a hydrothermal method, and then synthesizing a nano-flower-shaped vanadium-doped nickel phosphide material by a phosphating and roasting method. The specific process steps are as follows:

[0008] (1) Synthesis of nanoflower precursor by hydrothermal method: nickel nitrate hexahydrate, urea, and ammonium fluoride are weighed in a molar ratio of 2:6:1, and ammonium metavanadate is weighed in a molar ratio of 0.03-0.08 to nickel nitrate hexahydrate. The weighed materials are dissolved in deionized water and then transferred to a hydrothermal kettle with a polytetrafluoroethylene liner, and the volume ratio of deionized water to the capacity of the hydrothermal kettle is 70%. After sealing, the kettle is placed in a forced air oven at 115-125°C for reaction for 11.5-12.5h, and then cooled naturally to room temperature. The obtained product is fully filtered and washed with deionized water and anhydrous ethanol to make it neutral, and dried in a vacuum oven at 50-60°C for 7-9h;

[0009] (2) Phosphating and calcining to synthesize nanoflower-shaped vanadium-doped nickel phosphide materials: Weigh the synthesized precursor and NaH2PO2 in a mass ratio of 1:30 and place them in two high-temperature resistant corundum porcelain boats respectively. The high-temperature resistant corundum porcelain boat containing NaH2PO2 is placed upstream of the air inlet, and the high-temperature resistant corundum porcelain boat containing the precursor is placed downstream of the air inlet. Calcination is carried out in an Ar atmosphere, with the temperature rising from room temperature to 290-310°C at a heating rate of 2-4°C / min and heating for 1.5-2.5 hours, and then naturally cooling to room temperature.

[0010] The physical structure of electrocatalyst materials was tested using D8 Discover from Bruker, Germany. Figure 2 This is the X-ray diffraction (XRD) pattern of the material prepared in Example 2. The prepared material has a single phase and a phase structure of Ni2P. The energy dispersive spectrometer equipped with ZEISSGemini 300 was used to analyze the element distribution of the electrocatalyst material. Figure 3 , Figure 4 , Figure 5 The element surface scanning element distribution diagrams of the materials prepared in Example 3 show the presence and uniform distribution of V, Ni, and P elements in the materials. The lattice fringes of the electrocatalyst material were observed using JEM-2100-G20 from JEOL Co., Ltd. Figure 6 This is a high-resolution transmission electron microscopy image of the material prepared in Example 3. It can be observed that the lattice fringes of 0.22, 0.20, 0.34, and 0.51 nm of the material prepared in Example 3 correspond to the (111), (201), (001), and (100) planes of Ni2P. The stability of the electrocatalyst material was tested using CHI650D from Shanghai Chenhua Instrument Co., Ltd. Figure 7 This is the It curve of the material prepared in Example 3. It can be observed that the material prepared in Example 3 has strong stability within 24 hours. The microscopic morphology of the electrocatalyst material was tested using ZEISS Gemini 300. Figure 8 The SEM image of the material prepared for comparative example 3 shows that the microscopic morphology of the material is a three-dimensional nanoflower composed of two-dimensional nanosheets. The polarization curve of the electrocatalyst material was tested using CHI650D of Shanghai Chenhua Instrument Co., Ltd. to evaluate the electrocatalytic hydrogen evolution performance of the electrocatalyst material. The electrolyte used for the electrochemical performance test was 1.0 mol / L KOH (pH=14). A three-electrode system was used for electrochemical testing, with a glassy carbon electrode coated with a catalyst as the working electrode (WE), a graphite rod as the counter electrode (RE), and a saturated calomel electrode (SCE) as the reference electrode (CE). The measured electrode potential was calibrated with a reversible hydrogen electrode (RHE), Fig. 9 The hydrogen evolution curve of the prepared material is shown in Table 2. When the current density reaches 10 mA / cm 2When the overpotential of the material prepared in comparative example 1 is 191 mV, the overpotentials of the materials prepared in embodiment 1, embodiment 2, embodiment 3 and comparative example 2 are 148 mV, 137 mV, 86.3 mV and 171 mV respectively. It can be seen that the materials in the embodiments have a lower overpotential and have excellent electrochemical hydrogen evolution performance.

[0011] It can be seen that ammonium metavanadate is used as the vanadium source, an appropriate amount of vanadium element is introduced during the hydrothermal process, and the vanadium element is successfully incorporated into the Ni2P lattice during the phosphating roasting process.

[0012] The elemental composition of Example 1, Example 2, Example 3 and Comparative Example 2 was tested using an iCAP 7000Plus inductively coupled plasma spectrometer from Thermo Fisher Scientific, USA, and the results are shown in Table 1. The molar ratios of the elements in the final product were 0.03, 0.05, 0.08, and 0.11, respectively.

[0013] Table 1 Molar ratio of V and Ni in the materials prepared in the present embodiment and comparative example 2

[0014] Material V / Ni molar ratio Example 1 0.029 Example 2 0.047 Example 3 0.077 Comparative Example 2 0.11

[0015] V-Ni2P prepared by the method of the embodiment of the present invention and the comparative example method is used as an electrocatalyst for the hydrogen evolution reaction. It is ultrasonically treated with deionized water, isopropanol and Nafion to form a catalyst dispersion. The prepared dispersion is dropwise applied to the center of the treated glassy carbon electrode and dried naturally to form a film. The electrochemical performance test is carried out using a standard three-electrode system, that is, a glassy carbon electrode coated with a catalyst is used as the working electrode (WE), a graphite rod is used as the counter electrode (RE), and a saturated calomel electrode (SCE) is used as the reference electrode (CE). The measured electrode potential is calibrated with a reversible hydrogen electrode (RHE). The scanning potential range is 0.0V to -0.4V (vs. RHE), and IR correction (90%) is turned on. The LSV test is carried out at a scanning rate of 5mV / s. The test results are as follows: Figure 7 ,like Fig. 9 As shown, the vanadium-doped nickel phosphide prepared in Example 3 of the present invention has higher electrochemical activity for hydrogen evolution than that in Comparative Examples 1 and 2.

[0016] The characteristics and advantages of the method of the present invention are: (1) a precursor is prepared by a simple hydrothermal method, and the precursor can be prepared into a vanadium-doped nickel phosphide powder electrocatalytic hydrogen evolution material through phosphating and roasting. The synthesis method of the present invention is simple and has high controllability; (2) the method of the present invention can make vanadium uniformly doped into nickel phosphide during the phosphating and roasting process; (3) the vanadium-doped nickel phosphide electrocatalytic hydrogen evolution material prepared by the present invention has the advantages of uniform distribution, high hydrogen evolution activity and good stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a schematic diagram of the preparation process of vanadium-doped nickel phosphide.

[0018] Figure 2 This is an X-ray diffraction (XRD) diagram of the material prepared in Example 2 of the present invention. In the diagram, the abscissa is the diffraction angle 2θ, in degrees (°); the ordinate is the diffraction peak intensity, in absolute units (au).

[0019] Figure 3 This is a surface scanning element distribution diagram of the V element of the material prepared in Example 3 of the present invention.

[0020] Figure 4 This is a surface scanning element distribution diagram of the Ni element in the material prepared in Example 3 of the present invention.

[0021] Figure 5 This is a surface scanning element distribution diagram of the P element of the material prepared in Example 3 of the present invention.

[0022] Figure 6 This is a high-resolution transmission electron microscopy image of the material prepared in Example 3 of the present invention.

[0023] Figure 7 This is the chronoamperometric (It) curve of the material prepared in Example 3 of the present invention. In the figure, the horizontal axis is time, the unit is: hours; the vertical axis is the current density, the unit is: milliampere / square centimeter (mA / cm 2 ).

[0024] Figure 8 It is a scanning electron microscope (SEM) image of the material prepared in Comparative Example 1 of the present invention.

[0025] Fig. 9 The polarization curves of the materials prepared in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 of the present invention are shown in FIG. 1 . In the figure, the horizontal axis is the potential, the unit is: volt; the vertical axis is the current density, the unit is: milliampere / square centimeter (mA / cm 2 ).

[0026] In the figure, curve a is a polarization curve of the electro-catalytic hydrogen evolution material prepared in Example 1, curve b is a polarization curve of the electro-catalytic hydrogen evolution material prepared in Example 2, curve c is a polarization curve of the electro-catalytic hydrogen evolution material prepared in Example 3, curve d is a polarization curve of the electro-catalytic hydrogen evolution material prepared in Comparative Example 1, and curve e is a polarization curve of the electro-catalytic hydrogen evolution material prepared in Comparative Example 2. DETAILED DESCRIPTION

[0027] In order to further illustrate the technical solution of the present invention, the implementation scheme of the present invention is described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the technical solution of the present invention, rather than limiting the claims of the present invention.

[0028] Example 1

[0029] (1) 3mmol Ni(NO3)2·6H2O (0.87g), 0.09mmol NH4VO3 (0.011g), 9mmol urea (0.54g) and 1.5mmol NH4F (0.056g) were dissolved in 35mL deionized water to form a solution, which was then transferred to a hydrothermal autoclave with a 50mL polytetrafluoroethylene liner, sealed and placed in a forced air oven at 115°C for 12.5h, then naturally cooled to room temperature, and the obtained product was thoroughly filtered and washed with deionized water and anhydrous ethanol for 3 times each, and dried in a vacuum oven at 60°C for 7h to obtain a light yellow-green powder precursor 0.03V-Ni(OH)2. (x represents the molar ratio of V / Ni in the finished material).

[0030] (2) Weigh 50 mg of the synthesized 0.03V-Ni(OH)2 and 1.50 g of NaH2PO2 and place them in two high-temperature resistant corundum porcelain boats, respectively. The high-temperature resistant corundum porcelain boat containing NaH2PO2 is placed upstream of the air inlet, and the high-temperature resistant corundum porcelain boat containing 0.03V-Ni(OH)2 is placed downstream of the air inlet. They are calcined in an Ar atmosphere at a heating rate of 2°C / min from room temperature to 290°C and heated for 1.5 h. After naturally cooling to room temperature, a black powder 0.03V-Ni2P electrocatalytic hydrogen evolution material is obtained.

[0031] Figure 2 This is the XRD diagram of 0.03V-Ni2P prepared in this embodiment. It can be seen that no other diffraction peaks related to vanadium or vanadium phosphide species appear in the XRD diffraction peaks, indicating that the Ni2P electrocatalyst material has been successfully prepared. The 0.05V-Ni2P prepared in this embodiment was tested for overpotential at a scanning rate of 5mV / s under the test condition of pH=14. The test results are shown in Table 2. The overpotential of the 0.03V-Ni2P sample prepared in this embodiment of the present invention is 148mV.

[0032] Example 2

[0033] (1) 3mmol Ni(NO3)2·6H2O (0.87g), 0.15mmol NH4VO3 (0.018g), 9mmol urea (0.54g) and 1.5mmol NH4F (0.056g) were dissolved in 35mL deionized water to form a solution, which was then transferred to a hydrothermal autoclave with a 50mL polytetrafluoroethylene liner, sealed and placed in a forced air oven at 125°C for 11.5h, then naturally cooled to room temperature. The obtained product was thoroughly filtered and washed with deionized water and anhydrous ethanol for 3 times each, and dried in a vacuum oven at 55°C for 9h to obtain a light yellow-green powder 0.05V-Ni(OH)2.

[0034] (2) Weigh 50 mg of the synthesized 0.05V-Ni(OH)2 and 1.50 g of NaH2PO2 and place them in two high-temperature resistant corundum boats, respectively. The high-temperature resistant corundum boat containing NaH2PO2 is placed upstream of the air inlet, and the high-temperature resistant corundum boat containing 0.05V-Ni(OH)2 is placed downstream of the air inlet. The two boats are calcined in an Ar atmosphere at a heating rate of 4°C / min from room temperature to 310°C and heated for 2.5 hours. After cooling naturally to room temperature, a black powder 0.05V-Ni2P electrocatalytic hydrogen evolution material is obtained.

[0035] The 0.05V-Ni2P prepared in this embodiment was tested for overpotential at a scan rate of 5mV / s under the test condition of pH=14, and the test results are shown in Table 2. The overpotential of the 0.05V-Ni2P sample prepared in this embodiment of the present invention is 137mV.

[0036] Example 3

[0037] (1) 3mmol Ni(NO3)2·6H2O (0.87g), 0.21mmol NH4VO3 (0.025g), 9mmol urea (0.54g) and 1.5mmol NH4F (0.056g) were dissolved in 350mL deionized water to form a solution, which was then transferred to a hydrothermal autoclave with a 50mL polytetrafluoroethylene liner, sealed and placed in a forced air oven at 120°C for 12h, then naturally cooled to room temperature. The obtained product was thoroughly filtered and washed with deionized water and anhydrous ethanol for 3 times each, and dried in a vacuum oven at 50°C for 8h to obtain a light yellow-green powder precursor 0.08V-Ni(OH)2.

[0038] (2) Weigh 50 mg of the synthesized 0.08V-Ni(OH)2 and 1.50 g of NaH2PO2 and place them in two high-temperature resistant corundum porcelain boats, respectively. The high-temperature resistant corundum porcelain boat containing NaH2PO2 is placed upstream of the air inlet, and the high-temperature resistant corundum porcelain boat containing 0.08V-Ni(OH)2 is placed downstream of the air inlet. They are calcined in an Ar atmosphere at a heating rate of 3°C / min from room temperature to 300°C and heated for 2 hours. After naturally cooling to room temperature, a black powder 0.08V-Ni2P electrocatalytic hydrogen evolution material is obtained.

[0039] Figure 3 , 4 5 are mapping diagrams of 0.08V-Ni2P prepared in this embodiment. It can be observed that the elements of V, Ni, and P exist and are evenly distributed in 0.08V-Ni2P. Figure 6 From the HRTEM image of 0.08V-Ni2P prepared in this example, lattice fringes of 0.22, 0.20, 0.34, and 0.51 nm can be observed, corresponding to the (111), (201), (001), and (100) planes of Ni2P, indicating that V was successfully incorporated into the lattice of Ni2P. Figure 7 The It curve of 0.08V-Ni2P prepared in this embodiment shows that the 0.08V-Ni2P prepared in this embodiment has strong stability within 24 hours. The 0.08V-Ni2P prepared in this embodiment was tested for overpotential at a scan rate of 5mV / s under the test condition of pH=14, and the test results are shown in Table 2. The overpotential of the 0.08V-Ni2P sample prepared in this embodiment of the present invention is 86.3mV.

[0040] In order to further illustrate the effect and function of appropriate vanadium doping, electrocatalysts of nickel phosphide without vanadium doping and nickel phosphide doped with 11% vanadium were prepared for comparison.

[0041] Comparative Example 1

[0042] (1) 3mmol Ni(NO3)2·6H2O (0.87g), 9mmol urea (0.54g) and 1.5mmol NH4F (0.056g) were dissolved in 35mL deionized water to form a solution, which was then transferred to a hydrothermal autoclave with a 50mL polytetrafluoroethylene liner, sealed and placed in a forced air oven at 120°C for 12h, then naturally cooled to room temperature. The obtained product was thoroughly filtered and washed with deionized water and anhydrous ethanol for 3 times each, and dried in a vacuum oven at 50°C for 8h to obtain a light yellow-green powder precursor, denoted as Ni(OH)2.

[0043] (2) Weigh 50 mg of synthesized Ni(OH)2 and 1.50 g of NaH2PO2 and place them in two high-temperature resistant corundum porcelain boats, respectively. The high-temperature resistant corundum porcelain boat containing NaH2PO2 is placed upstream of the air inlet, and the high-temperature resistant corundum porcelain boat containing Ni(OH)2 is placed downstream of the air inlet. Calcination is performed in an Ar atmosphere, and the temperature is increased from room temperature to 300°C at a heating rate of 3°C / min and heated for 2 hours. After naturally cooling to room temperature, a black powder Ni2P electrocatalytic hydrogen evolution material is obtained.

[0044] Figure 8 This is a SEM image of the Ni2P prepared in this comparative example. It can be observed that the material is a nanoflower composed of nanosheets. The Ni2P prepared in this comparative example was tested for overpotential at a scan rate of 5mV / s under the test condition of pH=14. The test results are shown in Table 2. The overpotential of the 0.08V-Ni2P sample prepared by the method of the embodiment of the present invention is 191mV.

[0045] Comparative Example 2

[0046] (1) 3mmol Ni(NO3)2·6H2O (0.87g), 0.30mmol NH4VO3 (0.035g), 9mmol urea (0.54g) and 1.5mmol NH4F (0.056g) were dissolved in 35mL deionized water to form a solution, which was then transferred to a hydrothermal autoclave with a 50mL polytetrafluoroethylene liner, sealed and placed in a forced air oven at 120°C for 12h, then naturally cooled to room temperature. The obtained product was thoroughly filtered and washed with deionized water and anhydrous ethanol for 3 times each, and dried in a vacuum oven at 50°C for 8h to obtain a light yellow-green powder precursor recorded as 0.11V-Ni(OH)2.

[0047] (2) Weigh 50 mg of the synthesized 0.11V-Ni(OH)2 and 1.50 g of NaH2PO2 and place them in two high-temperature resistant corundum porcelain boats, respectively. The high-temperature resistant corundum porcelain boat containing NaH2PO2 is placed upstream of the air inlet, and the high-temperature resistant corundum porcelain boat containing 0.11V-Ni(OH)2 is placed downstream of the air inlet. They are calcined in an Ar atmosphere at a heating rate of 3°C / min from room temperature to 300°C and heated for 2 hours. After naturally cooling to room temperature, a black powder 0.11V-Ni2P electrocatalytic hydrogen evolution material is obtained.

[0048] The Ni2P prepared in this comparative example was tested for overpotential at a scan rate of 5 mV / s under the test condition of pH=14. The test results are shown in Table 2. The overpotential of the 0.11V-Ni2P sample prepared in this comparative example was 171 mV.

[0049] Table 2 Electrochemical hydrogen evolution performance of each embodiment and comparative example

[0050] name Overpotential (mV) Example 1 148 Example 2 137 Example 3 86.3 Comparative Example 1 191 Comparative Example 2 171

Claims

1. A vanadium-doped nickel phosphide electrocatalyst material, characterized in that: The catalyst material is composed of vanadium, nickel and phosphorus, and presents a Ni2P phase. Vanadium as a doping element does not form a separate phase. The molar ratio of vanadium to nickel is 0.03-0.08, and the molar ratio of nickel to phosphorus is 2:

1. The material is a three-dimensional nanoflower with a diameter distribution of 3-7 microns.

2. A method for preparing the vanadium-doped nickel phosphide electrocatalyst according to claim 1, characterized in that: Ammonium metavanadate is used as a vanadium source, a nano-flower-shaped precursor is synthesized by a hydrothermal method, and then a nano-flower-shaped vanadium-doped nickel phosphide material is synthesized by a phosphating and roasting method. The specific process steps are as follows: (1) Synthesis of nanoflower-like precursors by hydrothermal method: nickel nitrate hexahydrate, urea, and ammonium fluoride are weighed in a molar ratio of 2:6:1, and ammonium metavanadate is weighed in a molar ratio of 0.03-0.08 to nickel nitrate hexahydrate. The weighed materials are dissolved in deionized water and then transferred to a hydrothermal kettle with a polytetrafluoroethylene liner, and the volume ratio of deionized water to the capacity of the hydrothermal kettle is 70%. After sealing, the mixture is placed in a forced air oven at 115-125 degrees Celsius for reaction for 11.5-12.5 hours, and then naturally cooled to room temperature. The obtained product is fully filtered and washed with deionized water and anhydrous ethanol to make it neutral, and dried in a vacuum oven at 50-60 degrees Celsius for 7-9 hours; (2) Phosphating and calcining to synthesize nano-flower-shaped vanadium-doped nickel phosphide material: Weigh the synthesized precursor and NaH2PO2 in a mass ratio of 1:30 and place them in two high-temperature resistant corundum porcelain boats respectively. The high-temperature resistant corundum porcelain boat containing NaH2PO2 is placed upstream of the air inlet, and the high-temperature resistant corundum porcelain boat containing the precursor is placed downstream of the air inlet. Calcination is carried out in an Ar atmosphere, with the temperature rising from room temperature to 290-310 degrees Celsius at a heating rate of 2-4 degrees Celsius / min and heating for 1.5-2.5 hours, and then naturally cooling to room temperature.

Citation Information

Cited By

  • Preparation method of vanadium-nickel boride nanoparticle electro-catalytic material

    CN121321026A