Surface treatment method for aluminum alloy frame of photovoltaic module, photovoltaic module and photovoltaic system
The surface treatment of the aluminum alloy frame through the micro-arc oxidation process solves the problems of complex and high cost of the anodizing process, achieves dense bonding and good performance improvement of the ceramic film layer, and is suitable for large-scale production.
Patent Information
- Application Number
- CN202411123352.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the anodizing process of aluminum alloy frames is complicated, resulting in high production costs, and the ceramic film layer is not firmly bonded to the substrate, lacking good wear resistance, corrosion resistance and electrical insulation characteristics.
The surface treatment of aluminum alloy frames is carried out using micro-arc oxidation technology, including degreasing, micro-arc oxidation, cleaning, drying, and sealing steps, and the film forming agent of 10-20g/L and alkaline pH adjustment of 1-10g/L The electrolyte of the agent and 5-30g/L buffer has a current density of 5-15A/dm2, a pulse frequency of 400-1000Hz, a duty cycle of 10%-30%, and a positive and negative pulse ratio of 2.5-4.5:1 , the microarc oxidation time is 10-60 minutes.
It has achieved a firm combination of the ceramic film layer and the substrate, has a dense structure, improved microhardness, wear resistance, corrosion resistance, high temperature impact resistance and electrical insulation characteristics, reducing production costs and is suitable for large-scale industrial production.
Smart Images

Figure CN118996566A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and in particular to a surface treatment method for an aluminum alloy frame of a photovoltaic module, a photovoltaic module, and a photovoltaic system. Background Art
[0002] Photovoltaic modules (solar panels) are devices that absorb sunlight and convert solar radiation into electrical energy through the photoelectric effect. Photovoltaic modules generally consist of tempered glass, EVA, cells, backplanes and aluminum alloy frames, of which the aluminum alloy frames are used to support other components of the photovoltaic module. Therefore, the life of the aluminum alloy frame determines the upper limit of the life of the photovoltaic module.
[0003] In the prior art, in order to increase the life of the aluminum alloy frame, the surface of the aluminum alloy frame is usually treated by anodizing, thereby generating an oxide film layer with the characteristics of corrosion resistance, wear resistance, high temperature impact resistance and electrical insulation.
[0004] However, the conventional anodizing process is complicated, resulting in high production costs for surface treatment of the aluminum alloy frame.
[0005] It should be noted that the above content is not necessarily prior art, nor is it intended to limit the scope of patent protection of this application. Summary of the invention
[0006] The embodiments of the present application provide a surface treatment method for an aluminum alloy frame of a photovoltaic module, a photovoltaic module, and a photovoltaic system to solve or alleviate one or more of the technical problems raised above.
[0007] A first aspect of an embodiment of the present application provides a surface treatment method for an aluminum alloy frame of a photovoltaic module, comprising:
[0008] Degreasing the aluminum alloy frame of the photovoltaic module, and cleaning and drying the aluminum alloy frame after the degreasing process is completed;
[0009] Performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying;
[0010] Cleaning and drying the aluminum alloy frame after micro-arc oxidation treatment;
[0011] Performing a sealing process on the aluminum alloy frame that has been cleaned and dried again;
[0012] The components of the electrolyte for micro-arc oxidation treatment include 10-20 g / L of a film-forming agent, 1-10 g / L of an alkaline pH regulator, and 5-30 g / L of a buffer, wherein the film-forming agent is sodium phosphate or sodium silicate, the alkaline pH regulator is sodium hydroxide or potassium hydroxide, and the buffer is sodium citrate, potassium citrate, or sodium tungstate;
[0013] The process conditions of the micro-arc oxidation treatment are: the current density is 5-15A / dm 2 , the pulse frequency is 400-1000Hz, the duty cycle is 10%-30%, the positive and negative pulse ratio is (2.5-4.5):1, and the micro-arc oxidation time is 10-60min.
[0014] In one embodiment, the electrolyte solution further comprises 8-15 g / L of a colorant.
[0015] In one embodiment, the colorant is sodium vanadate or potassium dichromate;
[0016] Among them, when the colorant is potassium dichromate, the components of the electrolyte also include 5-10g / L of an additive and 8-15g / L of a complexing agent, the additive is sodium fluoride or potassium fluoride, the mass concentration ratio of the complexing agent to the colorant is 1:1, and the complexing agent is oxalic acid or sodium ethylenediaminetetraacetic acid.
[0017] In one embodiment, the degreasing treatment of the aluminum alloy frame of the photovoltaic module includes:
[0018] The aluminum alloy frame is degreased by using an acidic degreasing agent, wherein the acidic degreasing agent comprises a sulfuric acid solution or a phosphoric acid solution with a mass percentage concentration of 2-3%, and the degreasing treatment time is 3-5 minutes.
[0019] In one embodiment, sealing the aluminum alloy frame includes:
[0020] The aluminum alloy frame is sealed by a hot water sealing process, wherein the process conditions of the hot water sealing process are: water temperature is 95-100° C., pH value is 5.5-6, and sealing time is 10-30 minutes.
[0021] In one embodiment, the surface treatment further comprises:
[0022] The film-forming agent, the alkaline pH regulator and the buffer are added into deionized water or distilled water according to the concentration formula, and stirred evenly to obtain the electrolyte.
[0023] In one embodiment, after the step of sealing the aluminum alloy frame that has been cleaned and dried again, the step further includes:
[0024] The aluminum alloy frame after the sealing treatment is cleaned and dried.
[0025] In one embodiment, when the aluminum alloy frame is cleaned, the aluminum alloy frame is cleaned by multiple water washings, wherein the aluminum alloy frame is cleaned by deionized water or distilled water in the last water washing.
[0026] A second aspect of an embodiment of the present application provides an aluminum alloy frame for a photovoltaic module, which is formed by surface treatment of the aluminum alloy frame using the surface treatment method described above.
[0027] A third aspect of an embodiment of the present application provides a photovoltaic module, comprising the aluminum alloy frame for a photovoltaic module as described above.
[0028] The above technical solution adopted in the embodiment of the present application may have the following advantages:
[0029] In the embodiment of the present application, when the aluminum alloy frame of the photovoltaic module is subjected to surface treatment, a micro-arc oxidation process is adopted. Compared with the anodizing process, a large number of anodizing pre-treatment steps can be omitted, such as omitting the alkaline etching treatment, polishing treatment and cleaning treatment after the alkaline etching and polishing treatment of the aluminum alloy frame, thereby reducing the process flow and saving production costs. In addition, the embodiment of the present application adopts an electrolyte having a composition including 10-20g / L of a film-forming agent, 1-10g / L of an alkaline pH regulator and 5-30g / L of a buffer, and adopts a current density of 5-15A / dm 2 , the pulse frequency is 400-1000Hz, the duty cycle is 10%-30%, the positive and negative pulse ratio is (2.5-4.5): 1, and the micro-arc oxidation time is 10-60min. The micro-arc oxidation treatment is carried out under the process conditions. The obtained ceramic film layer can be firmly combined with the substrate, and the structure of the ceramic film layer is dense, and it has good wear resistance, corrosion resistance, high temperature impact resistance and electrical insulation properties, which can greatly improve the microhardness of the aluminum alloy frame. In addition, since the components of the electrolyte used are commonly used and low-cost compounds, the surface treatment method in this application is low-cost when surface treating the aluminum alloy frame, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.
[0031] Figure 1A flowchart of the steps of a surface treatment method for an aluminum alloy frame of a photovoltaic module provided in an embodiment of the present application. DETAILED DESCRIPTION
[0032] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. Wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.
[0033] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer or part discussed below can be represented as the second element, component, region, layer or part. And when the second element, component, region, layer or part is discussed, it does not mean that the present disclosure necessarily has the first element, component, region, layer or part.
[0034] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0035] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0036] It should be noted that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The orientation words "inside" and "outside" refer to the inside and outside relative to the outline of each component itself. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Therefore, the exemplary term "above..." can include both "above..." and "below..." orientations. The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here are interpreted accordingly.
[0037] In the present application, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values in the numerical interval is considered to be continuous, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to an integer in the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be merged. In other words, unless otherwise specified, the numerical range disclosed in the present application should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows for broadly including quantitative intervals such as percentage intervals, ratio intervals, and ratio intervals.
[0038] Hereinafter, exemplary embodiments according to the present application will be described in more detail with reference to the accompanying drawings. It should be noted that these exemplary embodiments can be implemented in many different forms and should not be construed as being limited to the embodiments described herein.
[0039] Explanation of the name of this application:
[0040] Micro-Arc Oxidation (MAO), also known as Plasma Electrolytic Oxidation (PEO), is an electrochemical surface treatment technology that generates a ceramic layer on the metal surface through a high-voltage current. The working principle of micro-arc oxidation is that under the action of a high-voltage electric field, the electrolyte interacts with the metal, causing a micro-arc discharge phenomenon on the metal surface, generating high temperature and high pressure. At the discharge point, the metal surface melts and reacts with the electrolyte to form a dense and hard ceramic oxide layer.
[0041] Anodic oxidation is a surface treatment technology that uses electrochemical methods to form an aluminum oxide film on the surface of aluminum and its alloys. The working principle of anodizing is to place the aluminum workpiece as an anode in an acidic electrolyte (such as sulfuric acid, oxalic acid or chromic acid), and a layer of oxide film is formed on the surface of the aluminum workpiece under the action of direct current in the electrolyte.
[0042] like Figure 1 As shown, the embodiment of the present application provides a surface treatment method for an aluminum alloy frame of a photovoltaic module. The preparation method may include:
[0043] Step S10, degreasing the aluminum alloy frame of the photovoltaic module, and cleaning and drying the aluminum alloy frame after the degreasing process is completed.
[0044] In the embodiment of the present application, the purpose of the degreasing treatment is to remove pollutants such as oil, dust, fingerprints, etc. on the surface of the aluminum alloy frame. When performing the degreasing treatment, chemical degreasing methods, solvent degreasing methods, etc. can be used. Among them, the chemical degreasing method includes using an alkaline solution or an acidic solution for degreasing treatment. The solvent degreasing method includes using an organic solvent to dissolve the grease for cleaning, and its implementation methods include scrubbing, immersion, spraying and ultrasonic cleaning.
[0045] The purpose of the cleaning process is to rinse off the residues of the degreasing process and the degreasing agent used for the degreasing process to ensure that there is no other residue on the aluminum alloy frame.
[0046] The purpose of the drying process is to remove the residual moisture in the cleaning process, ensure that the aluminum alloy frame is completely dry, and avoid moisture from entering the electrolyte, which affects the micro-arc oxidation process and the film quality. In this embodiment, the drying process can be achieved by cold air drying or natural air drying, which is not limited in this embodiment.
[0047] Step S11, performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying.
[0048] In an embodiment of the present application, when performing micro-arc oxidation treatment, the aluminum alloy frame is placed in an electrolytic cell of a micro-arc oxidation system, and the aluminum alloy frame is used as an anode, and a stainless steel or graphite rod is used as a cathode, and a bipolar pulse power supply is used for micro-arc oxidation treatment.
[0049] During the micro-arc oxidation treatment, the components of the electrolyte added to the electrolytic cell include 10-20 g / L (grams / liter) of a film-forming agent, 1-10 g / L (grams / liter) of an alkaline pH regulator, and 5-30 g / L (grams / liter) of a buffer.
[0050] The film-forming agent is used to react with the aluminum alloy to form a ceramic film during the micro-arc oxidation process. The film-forming agent can be sodium phosphate, sodium silicate or other phosphates and silicates. The mass concentration of the film-forming agent in the electrolyte is 10-20 g / L, including any point value within the mass concentration range, such as 10 g / L, 13 g / L, 17 g / L, and 20 g / L.
[0051] The alkaline pH regulator is used to adjust the pH value of the electrolyte, so that the electrolyte is alkaline, which is conducive to the surface oxidation of the aluminum alloy frame. The alkaline pH regulator can be a strong alkaline substance such as sodium hydroxide and potassium hydroxide. The mass concentration of the alkaline pH regulator in the electrolyte is 1-10g / L, including any point value within the mass concentration range, such as 1g / L, 5g / L, 7g / L, and 10g / L.
[0052] The buffer is used to adjust and stabilize the pH value of the electrolyte, prevent excessive dissolution of the oxide film, and improve the uniformity and stability of the film layer. The buffer can be sodium citrate, potassium citrate, sodium tungstate, or other citrates and tungstates. The mass concentration of the buffer in the electrolyte is 5-30 g / L, including any point value within the mass concentration range, such as 5 g / L, 15 g / L, 23 g / L, and 30 g / L.
[0053] During the micro-arc oxidation process, the process conditions are: current density is 5-15A / dm 2(ampere / square decimeter), the pulse frequency is 400-1000Hz (hertz), the duty cycle is 10%-30%, the positive and negative pulse ratio is (2.5-4.5): 1, and the micro-arc oxidation time is 10-60min (minutes).
[0054] The current density can be any value within the above current density range, for example, 5A / dm 2 、10A / dm 2 、13A / dm 2 、15A / dm 2 .
[0055] The pulse frequency may be any value within the above pulse frequency range, for example, 400 Hz, 600 Hz, 800 Hz, or 1000 Hz.
[0056] The duty cycle may be any value within the above duty cycle range, for example, 10%, 18%, 25%, or 30%.
[0057] The positive-to-negative pulse ratio may be any value within the above-mentioned positive-to-negative pulse ratio range, for example, 2.5:1, 3.5:1, 4.0:1, 4.5:1.
[0058] The micro-arc oxidation time can be any value within the above-mentioned micro-arc oxidation time range, for example, 10 min, 30 min, 45 min, 60 min.
[0059] Step S12, cleaning and drying the aluminum alloy frame after the micro-arc oxidation treatment.
[0060] In the embodiment of the present application, the purpose of cleaning the aluminum alloy frame after micro-arc oxidation is to remove the residues that may be generated on the surface of the aluminum alloy frame during the micro-arc oxidation process, such as unreacted electrolyte, oxide film fragments or other contaminants. In addition, cleaning the aluminum alloy frame after micro-arc oxidation also helps to ensure the cleanliness of the micro-arc oxidation film layer (ceramic film layer) and avoid the negative impact of the residue on the performance of the film layer, such as reducing the corrosion resistance or wear resistance of the film layer.
[0061] After the aluminum alloy frame that has been treated with micro-arc oxidation is completely cleaned, the aluminum alloy frame is dried. In the embodiment of the present application, the purpose of the drying process is to remove moisture from the surface of the aluminum alloy frame to prevent corrosion or oxidation caused by moisture, and also to prepare for subsequent sealing treatment.
[0062] Step S13, sealing the aluminum alloy frame that has been cleaned and dried again.
[0063] In the embodiment of the present application, the purpose of the pore sealing treatment is to fill and seal the micropores in the ceramic film layer formed after the micro-arc oxidation treatment, thereby effectively preventing the penetration of corrosive media and improving the corrosion resistance of the film layer. In addition, the pore sealing treatment can also improve the electrical insulation and wear resistance of the aluminum alloy frame surface.
[0064] When performing the sealing treatment, the aluminum alloy frame may be sealed using a hot water sealing process, a steam sealing process, a chemical sealing process, an organic sealing agent, or the like.
[0065] In the embodiment of the present application, when surface treatment is performed on the aluminum alloy frame of the photovoltaic module, the micro-arc oxidation process is adopted. Compared with the anodizing process, a large number of anodizing pre-treatment steps can be omitted, such as omitting the alkaline etching treatment, polishing treatment and cleaning treatment after the alkaline etching and polishing treatment of the aluminum alloy frame, thereby reducing the process flow and saving production costs. In addition, the embodiment of the present application adopts an electrolyte comprising 10-20g / L of a film-forming agent, 1-10g / L of an alkaline pH regulator and 5-30g / L of a buffer, and adopts a current density of 5-15A / dm 2 , the pulse frequency is 400-1000Hz, the duty cycle is 10%-30%, the positive and negative pulse ratio is (2.5-4.5): 1, and the micro-arc oxidation time is 10-60min. The micro-arc oxidation treatment is carried out under the process conditions. The obtained ceramic film layer can be firmly combined with the substrate, and the structure of the ceramic film layer is dense, and it has good wear resistance, corrosion resistance, high temperature impact resistance and electrical insulation properties, which can greatly improve the microhardness of the aluminum alloy frame. In addition, since the components of the electrolyte used are commonly used and low-cost compounds, the surface treatment method in this application is low-cost when surface treating the aluminum alloy frame, and is suitable for large-scale industrial production.
[0066] In one embodiment, in order to conveniently color the aluminum alloy frame, the electrolyte further comprises 8-15 g / L of a colorant.
[0067] In the embodiment of the present application, the colorant is used to form a colored ceramic film layer when forming the ceramic film layer. The specific composition of the colorant can be determined according to the required coloration. It is understandable that different coloring requirements correspond to different colorants.
[0068] The mass concentration of the colorant in the electrolyte is 8-15 g / L, including any point value within the mass concentration range, for example, 8 g / L, 10 g / L, 13 g / L, and 15 g / L.
[0069] In the embodiment of the present application, a colorant with a mass concentration of 8-15 g / L is added to the electrolyte, so that a colored ceramic film layer can be formed after the aluminum alloy frame is subjected to micro-arc oxidation treatment. Compared with the anodizing process, which requires additional coloring treatment to achieve the coloring of the aluminum alloy frame, the coloring method in the embodiment of the present application is more convenient and the coloring is more stable.
[0070] In one embodiment, when a dark or black ceramic film layer needs to be formed, the colorant can be other vanadates such as sodium vanadate and potassium vanadate.
[0071] In this embodiment, by adding vanadate with a mass concentration of 8-15 g / L into the electrolyte, a black ceramic film layer containing O, Al, Si, and V is formed after micro-arc oxidation of the aluminum alloy frame.
[0072] In one embodiment, when a green ceramic film layer needs to be formed, the colorant may be potassium dichromate.
[0073] In this embodiment, when potassium dichromate is used as a colorant, in order to form a green ceramic film layer, the components in the electrolyte further include additives and complexing agents.
[0074] The additive is used as a film-forming promoter, and can reduce the breakdown voltage, delay the ignition time, etc. The additive can be sodium fluoride, potassium fluoride, etc. The mass concentration of the additive in the electrolyte is 5-10g / L, including any point value within the mass concentration range, such as 5g / L, 6g / L, 8g / L, 10g / L.
[0075] The complexing agent is used to stabilize the electrolyte, prevent the precipitation or polymerization of metal ions, and improve the stability of the electrolyte. The complexing agent can be oxalic acid, sodium ethylenediaminetetraacetic acid, etc. The mass concentration of the complexing agent in the electrolyte is 8-15g / L, including any point value within the mass concentration range, such as 8g / L, 10g / L, 12g / L, and 15g / L. In addition, in this embodiment, the mass concentration ratio of the complexing agent to the colorant needs to be balanced according to 1:1, so that a green and stable ceramic film layer can be formed during micro-arc oxidation treatment.
[0076] In one embodiment, the degreasing treatment of the aluminum alloy frame of the photovoltaic module includes: using an acidic degreasing agent to degreasing the aluminum alloy frame, the acidic degreasing agent includes a sulfuric acid solution or a phosphoric acid solution with a mass percentage concentration of 2-3%, and the degreasing treatment time is 3-5 minutes.
[0077] In this embodiment, the percentage of the solute (sulfuric acid or phosphoric acid) in the sulfuric acid solution or the phosphoric acid solution to the entire solution mass can be any value between 2-3%, for example, 2%, 2.4%, 2.6%, 3%.
[0078] The degreasing treatment time can be any value within the above time range, for example, 3 minutes, 4 minutes, 4.5 minutes, or 5 minutes.
[0079] In this embodiment, the aluminum alloy frame is degreased by using an acidic degreasing agent containing a sulfuric acid solution or a phosphoric acid solution with a mass percentage concentration of 2-3%, and the degreasing time is controlled within 3-5 minutes, thereby ensuring that oil stains, fingerprints, etc. on the aluminum alloy frame are cleaned and avoiding excessive corrosion to the surface of the aluminum alloy frame.
[0080] In one embodiment, sealing the aluminum alloy frame includes: sealing the aluminum alloy frame using a hot water sealing process, wherein the process conditions of the hot water sealing process are: water temperature of 95-100°C, pH value of 5.5-6, and sealing time of 10-30 minutes.
[0081] In this embodiment, the aluminum alloy frame after micro-arc oxidation is sealed by using a hot water sealing process, so that water molecules can react with oxides in the ceramic film layer to form aluminum hydroxide, thereby sealing the micropores.
[0082] In this embodiment, the water temperature can be any value within the above temperature range, for example, 95°C, 97°C, 99°C, or 100°C.
[0083] The pH value may be any point within the above pH value range, for example, 5.5, 5.7, 5.8, 6. The pH value range may be adjusted by adding acetic acid to hot water.
[0084] The sealing time can be any point value within the above sealing time range, for example, 10min, 20min, 28min, 30min.
[0085] In the embodiment of the present application, the aluminum alloy frame after micro-arc oxidation is sealed by using a hot water sealing process. Compared with other sealing processes, the cost is lower and it is suitable for large-scale production.
[0086] In one embodiment, the surface treatment further comprises: adding the film-forming agent, the alkaline pH regulator and the buffer into deionized water or distilled water according to a concentration formula, and stirring evenly to obtain the electrolyte.
[0087] In this embodiment, when preparing the electrolyte, appropriate amounts of film-forming agent, alkaline pH regulator and buffer are selected according to a predetermined concentration formula and added to deionized water or distilled water, and then stirred evenly to obtain the required electrolyte formula.
[0088] As an example, the concentration formula is 15g / L of film-forming agent, 7g / L of alkaline pH regulator and 20g / L of buffer. When preparing the electrolyte, 15g of film-forming agent, 7g of alkaline pH regulator and 20g of buffer can be added to less than 1L (for example, 800mL) of deionized water or distilled water, and then stirred evenly so that all solutes are dissolved in the deionized water or distilled water. Finally, deionized water or distilled water is added to the electrolyte again until the electrolyte is 1L. At this time, the electrolyte with the above-mentioned concentration formula can be obtained.
[0089] In this embodiment, the electrolyte is prepared in advance, so that when the micro-arc oxidation treatment is performed, the prepared electrolyte can be directly used for the micro-arc oxidation treatment, thereby shortening the surface treatment process time.
[0090] In one embodiment, after the step of sealing the aluminum alloy frame that has been cleaned and dried again, the step further includes: cleaning and drying the aluminum alloy frame that has been sealed.
[0091] In the embodiment of the present application, the purpose of cleaning the aluminum alloy frame after the sealing process is to remove the sealing liquid that may remain on the surface of the aluminum alloy frame during the sealing process. In addition, the cleaning process can help ensure that the film layer after the sealing process is clean and avoid residues affecting the performance of the film layer, such as corrosion resistance or electrical insulation.
[0092] In the embodiment of the present application, after the aluminum alloy frame after the sealing treatment is cleaned, a drying treatment is performed to remove moisture on the surface of the aluminum alloy frame to prevent corrosion or oxidation caused by moisture.
[0093] During the drying process, the drying process may be carried out by natural air drying or by cold air drying. The specific treatment method is not limited in this embodiment.
[0094] In one embodiment, when the aluminum alloy frame is cleaned, the aluminum alloy frame may be cleaned by multiple water washings, wherein the aluminum alloy frame is cleaned by deionized water or distilled water during the last water washing.
[0095] In this embodiment, when the aluminum alloy frame is cleaned multiple times, in order to save costs, the previous cleaning process can be performed with tap water, but the last cleaning process needs to be performed with deionized water or distilled water to avoid the influence of ions in the water on subsequent processing processes.
[0096] In the embodiment of the present application, the residues can be cleaned as cleanly as possible through multiple cleaning operations, which is convenient for the processing in subsequent steps.
[0097] The following will conduct surface treatment on the aluminum alloy frame according to the surface treatment method of the aluminum alloy frame of the photovoltaic module provided in the following examples, and then conduct performance testing on the aluminum alloy frame with a ceramic film layer obtained after the surface treatment, and conduct performance testing on the aluminum alloy frame with an oxide film layer obtained by surface treatment of the aluminum alloy frame using the existing anodizing process, wherein the performance test parameters include corrosion current density, corrosion current and film layer microhardness, and the test results are shown in Table 1.
[0098] [Example 1]
[0099] A surface treatment method for an aluminum alloy frame of a photovoltaic module is as follows:
[0100] Step 1: Use an acidic degreasing agent to degrease the aluminum alloy frame. The main component of the degreasing agent is sulfuric acid, with a concentration of about 2.5%, and the degreasing time is 4 minutes.
[0101] Step 2: After degreasing, clean and dry the aluminum alloy frame.
[0102] Step 3: The aluminum alloy frame after cleaning and drying is subjected to micro-arc oxidation treatment, wherein the electrolyte composition of the micro-arc oxidation treatment includes 15g / L sodium silicate, 5g / L sodium hydroxide and 20g / L sodium citrate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10A / dm 2 , the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0103] Step 4: Clean and dry the aluminum alloy frame that has been treated with micro-arc oxidation.
[0104] Step 5: Use hot water sealing process to seal the aluminum alloy frame that has been cleaned and dried again, wherein the water temperature is 98° C., the pH is 5.8, and the sealing time is 30 minutes.
[0105] Step 6: Clean and dry the sealed aluminum alloy frame to obtain an aluminum alloy frame for testing.
[0106] [Example 2]
[0107] The aluminum alloy frame of Example 2 is treated by the surface treatment method of Example 1, except that step 3 of Example 2 is replaced by: performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying, wherein the composition of the electrolyte for micro-arc oxidation treatment includes 10 g / L sodium silicate, 5 g / L sodium hydroxide and 20 g / L sodium citrate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10 A / dm 2 , the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0108] [Example 3]
[0109] The aluminum alloy frame of Example 3 is treated by the surface treatment method of Example 1, except that step 3 of Example 3 is replaced by: performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying, wherein the composition of the electrolyte for micro-arc oxidation treatment includes 20 g / L sodium silicate, 5 g / L sodium hydroxide and 20 g / L sodium citrate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10 A / dm 2 , the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0110] [Example 4]
[0111] The aluminum alloy frame of Example 4 is treated by the surface treatment method of Example 4, except that step 3 of Example 4 is replaced by: performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying, wherein the composition of the electrolyte for micro-arc oxidation treatment includes 15 g / L sodium phosphate, 5 g / L sodium hydroxide and 20 g / L sodium citrate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10 A / dm 2 , the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0112] [Example 5]
[0113] The aluminum alloy frame of Example 5 is treated by the surface treatment method of Example 5, except that step 3 of Example 5 is replaced by: performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying, wherein the composition of the electrolyte for micro-arc oxidation treatment includes 15 g / L sodium silicate, 5 g / L sodium hydroxide and 5 g / L sodium citrate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10 A / dm 2, the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0114] [Example 6]
[0115] The aluminum alloy frame of Example 6 is treated by the surface treatment method of Example 6, except that step 3 of Example 6 is replaced by: performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying, wherein the composition of the electrolyte for micro-arc oxidation treatment includes 15 g / L sodium silicate, 5 g / L sodium hydroxide and 30 g / L sodium citrate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10 A / dm 2 , the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0116] [Example 7]
[0117] The aluminum alloy frame of Example 7 is treated by the surface treatment method of Example 7, except that step 3 of Example 7 is replaced by: performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying, wherein the composition of the electrolyte for micro-arc oxidation treatment includes 15 g / L sodium silicate, 5 g / L sodium hydroxide and 20 g / L potassium citrate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10 A / dm 2 , the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0118] [Example 8]
[0119] The aluminum alloy frame of Example 8 is treated by the surface treatment method of Example 8, except that step 3 of Example 8 is replaced by: performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying, wherein the composition of the electrolyte for micro-arc oxidation treatment includes 15 g / L sodium silicate, 5 g / L sodium hydroxide and 20 g / L sodium tungstate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10 A / dm 2 , the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0120] [Comparative Example 1]
[0121] The aluminum alloy frame of comparative example 1 is treated by the surface treatment method of embodiment 1, except that step 3 of comparative example 1 is replaced by: performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying, wherein the composition of the electrolyte for micro-arc oxidation treatment includes 5 g / L sodium silicate, 5 g / L sodium hydroxide and 20 g / L sodium citrate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10 A / dm 2 , the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0122] [Comparative Example 2]
[0123] The aluminum alloy frame of Comparative Example 1 is treated by the surface treatment method of Example 1, except that step 3 of Comparative Example 1 is replaced by: performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying, wherein the composition of the electrolyte for micro-arc oxidation treatment includes 25 g / L sodium silicate, 5 g / L sodium hydroxide and 20 g / L sodium citrate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10 A / dm 2 , the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0124] [Comparative Example 3]
[0125] The aluminum alloy frame of Comparative Example 3 is treated by the surface treatment method of Example 1, except that step 3 of Comparative Example 3 is replaced by: performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying, wherein the composition of the electrolyte for micro-arc oxidation treatment includes 15 g / L sodium silicate, 5 g / L sodium hydroxide and 2 g / L sodium citrate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10 A / dm 2 , the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0126] [Comparative Example 4]
[0127] The aluminum alloy frame of Comparative Example 4 is treated by the surface treatment method of Example 1, except that step 3 of Comparative Example 3 is replaced by: performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying, wherein the composition of the electrolyte for micro-arc oxidation treatment includes 15 g / L sodium silicate, 5 g / L sodium hydroxide and 40 g / L sodium citrate, and the process conditions of the micro-arc oxidation treatment are: the current density is 10 A / dm 2 , the pulse frequency is 800 Hz, the duty cycle is 20%, the positive and negative pulse ratio is 3.5:1, and the micro-arc oxidation time is 40 min.
[0128] [Comparative Example 5]
[0129] A surface treatment method for an aluminum alloy frame of a photovoltaic module is as follows:
[0130] Step 1: Use an acidic degreasing agent to degrease the aluminum alloy frame. The main component of the degreasing agent is sulfuric acid, with a concentration of about 2.5%, and the degreasing time is 4 minutes.
[0131] Step 2: After degreasing, clean the aluminum alloy frame.
[0132] Step 3: Place the cleaned aluminum alloy frame in an alkaline etching solution for alkaline etching.
[0133] Step 4: Clean the aluminum alloy frame after alkaline etching.
[0134] Step 5: Perform alkali polishing on the aluminum alloy frame.
[0135] Step 6: Clean the aluminum alloy frame.
[0136] Step 7: placing the aluminum alloy frame in an electrolyte for anodizing treatment, wherein the electrolyte comprises sulfuric acid with a concentration of 15%, and the process conditions of anodizing are: current density: 4A / dm2, voltage 70V, temperature 5°C, and time 120min.
[0137] Step 8: Clean and dry the anodized aluminum alloy frame.
[0138] Step 9: Use hot water sealing technology to seal the aluminum alloy frame, wherein the water temperature is 98° C., the pH is 5.8, and the sealing time is 30 minutes.
[0139] Step 10: Clean and dry the sealed aluminum alloy frame to obtain an aluminum alloy frame for testing.
[0140] Table 1: Test results of aluminum alloy frame
[0141]
[0142] By comparison, it can be seen that the aluminum alloy frame treated by the surface treatment method in Examples 1-8 has a higher Vickers hardness than the aluminum alloy frame obtained by anodizing process in Comparative Example 5, and the corrosion potential in most of the embodiments in Examples 1-8 is also higher than the corrosion potential in Comparative Example 5, indicating that after the aluminum alloy frame is treated by a suitable micro-arc oxidation process, it has better corrosion resistance than the aluminum alloy frame obtained by anodizing process.
[0143] The embodiment of the present application may also provide an aluminum alloy frame for a photovoltaic module, which is formed by surface treating the aluminum alloy frame using the surface treatment method in the above embodiment.
[0144] The embodiment of the present application may also provide a photovoltaic assembly (not shown), wherein the photovoltaic assembly includes the aluminum alloy frame for the photovoltaic assembly described above.
[0145] The embodiment of the present application can provide a photovoltaic system, including the photovoltaic components in any of the above embodiments. The advantages of the above photovoltaic components are also possessed by the photovoltaic system, which will not be repeated here. The above photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is to say, the photovoltaic system can be used in all fields where solar energy is required for power generation. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components may form multiple photovoltaic arrays. The photovoltaic array is connected to a junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to realize solar power supply.
[0146] It should be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Furthermore, when describing a specific feature, structure or characteristic in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.
[0147] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0148] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A surface treatment method for an aluminum alloy frame of a photovoltaic module, characterized in that: include: Degreasing the aluminum alloy frame of the photovoltaic module, and cleaning and drying the aluminum alloy frame after the degreasing process is completed; Performing micro-arc oxidation treatment on the aluminum alloy frame after cleaning and drying; Cleaning and drying the aluminum alloy frame after micro-arc oxidation treatment; Performing a sealing process on the aluminum alloy frame that has been cleaned and dried again; The components of the electrolyte for micro-arc oxidation treatment include 10-20 g / L of a film-forming agent, 1-10 g / L of an alkaline pH regulator, and 5-30 g / L of a buffer, wherein the film-forming agent is sodium phosphate or sodium silicate, the alkaline pH regulator is sodium hydroxide or potassium hydroxide, and the buffer is sodium citrate, potassium citrate, or sodium tungstate; The process conditions of the micro-arc oxidation treatment are: the current density is 5-15A / dm 2 , the pulse frequency is 400-1000Hz, the duty cycle is 10%-30%, the positive and negative pulse ratio is (2.5-4.5):1, and the micro-arc oxidation time is 10-60min.
2. The surface treatment method according to claim 1, characterized in that: The electrolyte also includes 8-15 g / L of a colorant.
3. The surface treatment method according to claim 2, characterized in that: The colorant is sodium vanadate or potassium dichromate; Among them, when the colorant is potassium dichromate, the components of the electrolyte also include 5-10g / L of an additive and 8-15g / L of a complexing agent, the additive is sodium fluoride or potassium fluoride, the mass concentration ratio of the complexing agent to the colorant is 1:1, and the complexing agent is oxalic acid or sodium ethylenediaminetetraacetic acid.
4. The surface treatment method according to any one of claims 1 to 3, characterized in that: The degreasing treatment of the aluminum alloy frame of the photovoltaic module comprises: The aluminum alloy frame is degreased by using an acidic degreasing agent, wherein the acidic degreasing agent comprises a sulfuric acid solution or a phosphoric acid solution with a mass percentage concentration of 2-3%, and the degreasing treatment time is 3-5 minutes.
5. The surface treatment method according to any one of claims 1 to 3, characterized in that: The sealing process for the aluminum alloy frame includes: The aluminum alloy frame is sealed by a hot water sealing process, wherein the process conditions of the hot water sealing process are: water temperature is 95-100° C., pH value is 5.5-6, and sealing time is 10-30 minutes.
6. The surface treatment method according to claim 1, characterized in that: The surface treatment also includes: The film-forming agent, the alkaline pH regulator and the buffer are added into deionized water or distilled water according to the concentration formula, and stirred evenly to obtain the electrolyte.
7. The surface treatment method according to claim 1, characterized in that: After the step of sealing the aluminum alloy frame that has been cleaned and dried again, the method further includes: The aluminum alloy frame after the sealing treatment is cleaned and dried.
8. The surface treatment method according to claim 1, characterized in that: When the aluminum alloy frame is cleaned, the aluminum alloy frame is cleaned by multiple water washings, wherein the aluminum alloy frame is cleaned by deionized water or distilled water during the last water washing.
9. An aluminum alloy frame for a photovoltaic module, characterized in that: The aluminum alloy frame is surface treated by the surface treatment method according to any one of claims 1 to 8.
10. A photovoltaic module, characterized in that: The photovoltaic module comprises the aluminum alloy frame for photovoltaic modules as claimed in claim 9.