Method for controlling copper thickness of electroplating hole filling surface of glass-based packaging carrier plate

Through segmented electroplating and the use of polyquaternary ammonium compounds, the complex problems of metal layer curling and copper reduction processes in glass through-hole technology are solved, and the effect of surface copper thickness control and copper filling in the hole is achieved, which improves the reliability of the product and simplicity of craftsmanship.

CN118996591APending Publication Date: 2024-11-22KUN SHAN FRJ TECH LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411180094.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In glass through-hole technology, the metal layer is prone to curling or falling off during the electroplating and filling process, and the existing copper reduction process is costly and complex, which affects the product's excellent rate.

Method used

The segmented electroplating method is adopted to control the copper thickness by alternating the forward and reverse pulse currents, and polyquaternary ammonium salt compound is added to the plating solution to improve the copper deposition efficiency and uniformity.

Benefits of technology

Effectively control the thickness of copper on the surface, reduce production costs, improve product yield, ensure that the copper in the hole is full and not easy to fall off, and is suitable for optical communication, radio frequency, micro-electromechanical systems and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996591A_ABST
    Figure CN118996591A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of processing of glass serving as a packaging carrier plate, and particularly relates to a method for controlling the copper thickness of an electroplating hole filling surface of a glass-based packaging carrier plate, which comprises the following steps of: (1) forming a through hole in the glass-based packaging carrier plate; (2) vacuum sputtering: plating a layer of copper or copper alloy on the surface of the glass-based packaging carrier plate and the surfaces of the holes by adopting a sputtering method; and (3) electroplating and hole filling are conducted, specifically, segmented electroplating is adopted, six or seven electroplating current segments are included in the electroplating process, the electroplating current is direct current, and the thickness of surface copper electroplated on the surface of the glass-based packaging carrier plate is reduced through alternate switching of forward pulse current and reverse pulse current from the third segment. According to the method, the hole can be filled, the copper thickness of the hole can be guaranteed, meanwhile, the surface copper can be controlled to be thin, subsequent fine circuit manufacturing is facilitated, a traditional chemical or mechanical copper reduction process is not needed in the subsequent process, and the production cost is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The patent of this invention belongs to the technical field of processing glass as a packaging substrate, and specifically relates to a method for controlling the copper thickness of the electroplated hole filling surface of a glass-based packaging substrate. Background Art

[0002] Through Silicon Via (TSV) technology is a high-density packaging technology that achieves vertical electrical interconnection of silicon vias by filling conductive materials such as copper, tungsten, and polysilicon. At present, through silicon via technology (TSV) is relatively mature and has been widely used in actual production, but silicon is a semiconductor material. Under the action of electric or magnetic fields, the carriers around it can move freely, which may interfere with adjacent circuits or signals, thereby affecting the performance of the chip. Therefore, the cost of silicon-based adapters is high and the electrical performance is poor, which limits their market application.

[0003] Glass materials have excellent dielectric properties, a thermal expansion coefficient close to that of silicon, and good mechanical stability. Even at very thin thicknesses, warping is very small. In addition, large-size glass panels are easy to obtain, which reduces process complexity and processing costs, and does not require the production of insulating layers. Therefore, through-glass vias (TGVs) and related technologies have broad application prospects in optical communications, radio frequency, microwaves, microelectromechanical systems, microfluidic devices, and three-dimensional integration. They are expected to replace TSV in some scenarios and become one of the core evolution directions of advanced packaging in the AI ​​era.

[0004] Up to now, the main difficulties in the development of glass through-hole 3D interconnection technology include: 1) Compared with silicon materials, due to the smooth surface of glass, the adhesion with common metals (such as Cu) is poor, which easily causes the delamination between the glass substrate and the metal layer, resulting in the curling of the metal layer and even falling off; 2) High-quality filling technology of TGV. Unlike TSV, the aperture of TGV is relatively large and most of them are through holes. In the electroplating filling process of the existing technology, with the deposition of copper ions in the hole, the thickness of the surface copper plating layer has been increasing. For the subsequent fine circuit production, the surface copper thickness needs to be reduced to below the required thickness of the circuit. For the second technical difficulty, that is, the high-quality filling technology of TGV, chemical micro-etching or mechanical copper reduction (mechanical grinding) is usually used to reduce the surface copper thickness. However, chemical micro-etching to reduce copper is prone to uneven surface copper thickness, and mechanical grinding to reduce copper is prone to hole cracks. It can be seen that whether chemical etching or mechanical grinding to reduce copper has high costs, complex processes, and is prone to reduce product quality. Summary of the invention

[0005] The purpose of the present invention is to provide a method for controlling the thickness of surface copper in electroplating hole filling of a glass-based packaging substrate, which can fill the hole and ensure the hole copper thickness, while also controlling the surface copper to a thinner thickness, which is beneficial to the subsequent fine circuit production, and does not require the subsequent traditional chemical or mechanical copper reduction process, effectively reducing the production cost.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A method for controlling the copper thickness of a glass-based package substrate electroplating hole filling surface comprises the following steps:

[0008] (1) forming a through hole on a glass-based packaging substrate;

[0009] (2) Vacuum sputtering: A layer of copper or copper alloy is plated on the surface of the glass-based package substrate and the surface of the hole by sputtering;

[0010] (3) Electroplating hole filling: segmented electroplating is adopted, and the electroplating current is direct current. From the third segment, positive and reverse pulse currents are alternately switched to reduce the thickness of the surface copper plated on the surface of the glass-based package substrate. The details are as follows:

[0011] The first stage: forward current electroplating, current density is 1ASf, time is 10~15min;

[0012] The second stage: forward current electroplating, current density is 2ASf, time is 30~60min;

[0013] The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100-150ms, the forward and reverse pulse time ratio is (2:1)-(4:1), and the total electroplating time of the third stage current is 5-120min;

[0014] The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50 to 100ms, the forward and reverse pulse time ratio is (1:1) to (2:1), and the total electroplating time of the fourth stage current is 60 to 180min;

[0015] The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30 to 50ms, the forward and reverse pulse time ratio is (1:2) to (2:1), and the total electroplating time of the fifth stage current is 10 to 120min;

[0016] The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20 to 30ms, the forward and reverse pulse time ratio is (1:1) to (1:3), and the total electroplating time of the sixth stage current is 60 to 120min;

[0017] The seventh stage: the current density is 3-5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20-30ms, the forward and reverse pulse time ratio is (1:1)-(1:3), and the total electroplating time of the seventh stage current is greater than or equal to 0min and less than or equal to 60min;

[0018] The plating solution used in electroplating includes a solution containing copper ions and other organic additives.

[0019] In the present invention, six or seven electroplating current sections are included in the electroplating process. The present invention can save electroplating time, improve electroplating efficiency, and effectively control the surface copper thickness while filling the hole. In addition, the current density used in the electroplating process of the present invention is relatively small as a whole, which can help make copper more compact. Wherein, the first section electroplating current density is small, and in the first section electroplating process, there is basically no copper deposition on the hole and the plate surface of the glass substrate. The main function of the first section electroplating is to discharge the bubbles (hydrogen) in the hole by vibration, and at the same time, the surface of the glass substrate and the through hole are soaked and wetted by the jet, so as to facilitate the subsequent electroplating reaction and the deposition of copper. Starting from the second section electroplating, copper deposition is gradually formed on the plate surface of the hole and the glass substrate respectively. The second section electroplating is only forward current electroplating, which can save electroplating time, improve electroplating efficiency, and is conducive to the rapid growth of hole copper. When the hole copper is deposited to a certain extent, the surface copper has also been deposited to a certain thickness. By continuously switching the current direction, under the action of the reverse pulse current, the surface copper will be dissolved, thereby making the surface copper thinner. The copper on the surface of the hole mouth may also be partially dissolved during the reverse current, but because the hole is a low current density area, and the reverse current is a pulse current with a shorter time (it will soon switch to a forward current), the copper in the hole will continue to be deposited and will hardly be dissolved. Therefore, the present invention can ensure that the copper in the hole is getting thicker and thicker while thinning the surface copper. Usually, in the entire electroplating process, the total time of the fourth section electroplating is the longest. At the end of the fourth section electroplating set by the present invention, the copper in the hole is about to be filled or has been basically filled and filled. The main function of the fifth to seventh sections of electroplating is to thin the thickness of the surface copper and make the copper in the hole continue to fill and fill. The present invention uses multi-segment pulse electroplating to reasonably design the forward and reverse current density and time, so that the copper layer in the hole becomes thicker and thicker, making it difficult to fall off, and at the same time, the surface copper can be made thinner and thinner, reducing the thickness of the surface copper, which is beneficial to the subsequent fine circuit production.

[0020] The size (especially the thickness), aspect ratio, number of holes, hole diameter, hole area, and side strips of the glass substrate (i.e., glass-based packaging carrier) will all affect the electroplating effect. Among them, the aspect ratio is the ratio of the thickness of the board to the hole diameter. When the aspect ratio is different, the difficulty coefficient of electroplating is different.

[0021] When the difficulty coefficient of electroplating hole filling is low, for example, the glass substrate is thin, and / or the aspect ratio does not exceed 6:1, the electroplating time of the third and / or fifth sections can be shorter. As a preferred embodiment, the electroplating hole filling operation can be: using segmented electroplating, the electroplating process includes six current sections, the electroplating current is direct current, and starting from the third section, the forward and reverse pulse currents are alternately switched to reduce the thickness of the surface copper electroplated on the surface of the glass-based package carrier, as follows:

[0022] The first stage: forward current electroplating, current density is 1ASf, time is 10min;

[0023] The second stage: forward current electroplating, current density is 2ASf, time is 30~50min;

[0024] The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100-150ms, the forward and reverse pulse time ratio is (2:1)-(4:1), and the total electroplating time of the third stage current is 5-60min;

[0025] The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50 to 100ms, the forward and reverse pulse time ratio is (1:1) to (2:1), and the total electroplating time of the fourth stage current is 60 to 90min;

[0026] The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30 to 50ms, the forward and reverse pulse time ratio is (1:1) to (1:2), and the total electroplating time of the fifth stage current is 20 to 80min;

[0027] The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20 to 30ms, the forward and reverse pulse time ratio is (1:1) to (1:2), and the total electroplating time of the sixth stage current is 60 to 80min.

[0028] When the difficulty coefficient of electroplating hole filling is slightly higher and the surface copper thickness is not easy to control at a thinner thickness, such as when the board is thicker and / or the aspect ratio is about 10:1, the electroplating hole filling operation is preferably: segmented electroplating is adopted, and the electroplating process includes six current segments, and the electroplating current is direct current, wherein from the third segment, positive and reverse pulse currents are alternately switched to reduce the thickness of the surface copper plated on the surface of the glass-based package substrate, as follows:

[0029] The first stage: forward current electroplating, current density is 1ASf, time is 10min;

[0030] The second stage: forward current electroplating, current density is 2ASf, time is 50-60min;

[0031] The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100-150ms, the forward and reverse pulse time ratio is (2:1)-(4:1), and the total electroplating time of the third stage current is 70-100min;

[0032] The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50 to 100ms, the forward and reverse pulse time ratio is (1:1) to (2:1), and the total electroplating time of the fourth stage current is 100 to 150min;

[0033] The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30 to 50ms, the forward and reverse pulse time ratio is (1:1) to (1:2), and the total electroplating time of the fifth stage current is 60 to 120min;

[0034] The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20 to 30ms, the forward and reverse pulse time ratio is (1:1) to (1:3), and the total electroplating time of the sixth stage current is 90 to 120min.

[0035] When the difficulty coefficient of electroplating hole filling is high, and the surface copper is difficult to control within a thin range when the hole is filled, for example, when the board thickness is greater than or equal to 700 μm, and / or the aspect ratio exceeds 15:1, the total electroplating time of the fifth segment during electroplating hole filling can be shorter (or even omitted). As a preferred embodiment, the electroplating hole filling operation can be: adopting segmented electroplating, the electroplating process includes seven current segments, the electroplating current is direct current, wherein starting from the third segment, positive and reverse pulse currents are alternately switched to reduce the thickness of the surface copper electroplated on the surface of the glass-based package carrier, as follows:

[0036] The first stage: forward current electroplating, current density is 1ASf, time is 10min;

[0037] The second stage: forward current electroplating, current density is 2ASf, time is 40~60min;

[0038] The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100-150ms, the forward and reverse pulse time ratio is (2:1)-(4:1), and the total electroplating time of the third stage current is 100-120min;

[0039] The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50 to 100ms, the forward and reverse pulse time ratio is (1:1) to (2:1), and the total electroplating time of the fourth stage current is 130 to 180min;

[0040] The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30 to 50ms, the forward and reverse pulse time ratio is (1:2) to (2:1), and the total electroplating time of the fifth stage current is 10 to 80min;

[0041] The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20 to 30ms, the forward and reverse pulse time ratio is (1:1) to (1:2), and the total electroplating time of the sixth stage current is 80 to 120min;

[0042] The seventh stage: the current density is 3-5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20-30ms, the forward and reverse pulse time ratio is (1:1)-(1:3), and the total electroplating time of the seventh stage current is 40-60min.

[0043] Furthermore, during the first and second electroplating stages, a mobile spray plate or cathode plate is reciprocated to effectively ensure uniform ion concentration distribution at various locations within the TGV hole, reduce the effective thickness of the diffusion layer, and thereby improve copper deposition efficiency.

[0044] Furthermore, forming through holes on a glass-based packaging carrier can be accomplished by laser-induced modification and acid etching, and the specific steps are as follows: a pulsed laser beam is focused into a laser beam focal line and irradiated onto a glass substrate, the laser beam focal line generates induced absorption within the glass substrate, so that the laser beam focal line generates a defect line extending through the thickness of the glass substrate at the irradiated position, and the glass substrate irradiated with the laser beam is placed in a hydrofluoric acid solution to etch holes, which has the advantage of avoiding cracks caused by laser peeling.

[0045] Further, the sputtering is carried out by a pulse power supply, the operating voltage is between 400 volts and 700 volts, and the thickness of the copper or copper alloy sputtered on the surface of the glass-based packaging carrier and the surface of the hole is 400-800nm. Due to the conductivity of the metal, sputtering copper or copper alloy on the glass surface and the surface of the hole is to facilitate the subsequent electroplating deposition step. Since the glass surface is smooth and has poor adhesion to copper, it is easy to cause stratification between the glass substrate and the metal layer, resulting in curling of the metal layer, or even falling off. As a preferred embodiment, the sputtering on the glass surface and the hole surface is an alloy of copper, nickel, and zinc, wherein the mass fraction of copper is 75-80%, the mass fraction of nickel is 15-21%, and the mass fraction of zinc is 2-5%. Compared with copper plating, the copper alloy (alloy of copper, nickel, and zinc) of the present invention can improve adhesion, enhance electroplating effect, facilitate copper ion deposition in the hole, and reduce the occurrence of curling and even falling off of the electroplated metal layer.

[0046] Furthermore, in the electroplating solution, the solution containing copper ions can be a copper sulfate solution; the organic additive can include a thiadiazole amide compound and / or a polyquaternary ammonium salt compound with a molecular weight greater than 3000, preferably a polyquaternary ammonium salt compound with a molecular weight greater than 3000. By adding the polyquaternary ammonium salt compound and / or the thiadiazole amide compound to the solution, the growth of the pore copper and the control of the thickness of the surface copper can be facilitated. The polyquaternary ammonium salt compound is preferably a reaction product of an ether containing a tertiary amine structure and tetrachloromethylmethane, and the effect is best when the dosage is 50 to 150 mg / L. Since the polyquaternary ammonium salt of the present invention is an alternating copolymer of an ether containing a tertiary amine structure and tetrachloromethylmethane, it contains a highly branched dendritic structure and has good water solubility, and since the macromolecular polymer is relatively difficult to enter the pore, the number of complexed copper ions in the pore is relatively small, thereby increasing the copper plating speed in the pore, which can be beneficial to the growth of the pore copper and the control of the thickness of the surface copper, and the deep plating effect is good. In addition, the above-mentioned polyquaternary ammonium salt leveler can improve the dispersibility and covering ability of the plating solution. Since the amine functional groups carry positive charges, they are easily adsorbed in high current density areas, especially in protruding areas on the board surface (where the copper is thicker), thereby reducing copper deposition in these areas, making the coating surface more uniform and making the coating denser.

[0047] Furthermore, the organic additive may also include an accelerator, or an accelerator and a wetting agent. Preferably, the wetting agent is a polymer compound containing an ether bond, or a homopolymer block copolymer of ethylene oxide and propylene oxide.

[0048] Furthermore, the electroplating temperature is 20-30°C.

[0049] The above-mentioned method for controlling the copper thickness of the electroplating hole filling surface of the present invention is not only applicable to through holes, but also to blind holes.

[0050] A glass product prepared according to the method can be applied to optical communication, radio frequency, microwave, micro-electromechanical system, microfluidic device and three-dimensional integration fields and MEMS packaging fields, etc.

[0051] Specifically, compared with the prior art, this technology can produce the following positive effects: the present invention can improve the distribution of hole copper and surface copper thickness, and through multi-stage pulse electroplating, reasonably design the forward and reverse current density and time, it can ensure the thickness of hole copper, fill the hole, and prevent it from falling off, while also controlling the surface copper to a thinner thickness, which is beneficial to the subsequent fine circuit production. In addition, since the present invention does not require a subsequent copper reduction process, it reduces production costs and makes the copper surface more uniform and flat, so the present invention has a high yield rate, more reliable quality, and a simpler process. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1The present invention is a flow chart of a method for controlling the copper thickness of a hole-filling surface of a glass-based packaging substrate electroplating.

[0053] Figure 2 This is a hole filling effect diagram of Example 5 (Part 1);

[0054] Figure 3 This is the hole filling effect diagram of Example 5 (Part 2);

[0055] Figure 4 This is a hole filling effect diagram of Example 6;

[0056] Figure 5 This is a diagram showing the hole filling effect of Example 7. DETAILED DESCRIPTION

[0057] The following examples are provided to facilitate a better understanding of the present invention, but are not intended to limit the present invention. The experimental methods in the following examples are conventional methods unless otherwise specified.

[0058] Example 1

[0059] In this embodiment, the glass substrate has a thickness of 388.2 μm, a minimum aperture of 92.6 μm, and an aspect ratio of about 4.2:1. The method for controlling the surface copper thickness during the electroplating hole filling process includes the following steps:

[0060] (1) forming a through hole on a glass-based packaging substrate;

[0061] (2) Vacuum sputtering: A layer of copper or copper alloy is plated on the surface of the glass-based package substrate and the surface of the hole by sputtering;

[0062] (3) Electroplating hole filling: segmented electroplating is adopted, and the electroplating process includes six stages of electroplating. From the first stage to the sixth stage, the electroplating current is direct current. From the third stage, positive and reverse pulse currents are alternately switched to reduce the thickness of the surface copper electroplated on the surface of the glass-based package substrate. The details are as follows:

[0063] The first stage: forward current electroplating, current density is 1ASf, time is 10min;

[0064] The second stage: forward current electroplating, current density is 2ASf, time is 45min;

[0065] The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100ms, the forward and reverse pulse time ratio is 2:1, and the total electroplating time of the third stage current is 35min;

[0066] The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time can be 100ms, the forward and reverse pulse time ratio is 2:1, and the total electroplating time of the fourth stage current is 70min;

[0067] The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50ms, the forward and reverse pulse time ratio is 1:2, and the total electroplating time of the fifth stage current is 20min;

[0068] The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30ms, the forward and reverse pulse time ratio is 1:1.5, and the total electroplating time of the sixth stage current is 65min;

[0069] The plating solution used in electroplating includes a solution containing copper ions and other organic additives.

[0070] Example 2

[0071] In this embodiment, the glass substrate has a thickness of 425 μm, a minimum aperture of 70 μm, and an aspect ratio of 6:1. The method for controlling the surface copper thickness during the electroplating hole filling process includes the following steps:

[0072] (1) forming a through hole on a glass-based packaging substrate;

[0073] (2) Vacuum sputtering: A layer of copper or copper alloy is plated on the surface of the glass-based package substrate and the surface of the hole by sputtering;

[0074] (3) Electroplating hole filling: segmented electroplating is adopted, and the electroplating process includes six stages of electroplating. From the first stage to the sixth stage, the electroplating current is direct current. From the third stage, positive and reverse pulse currents are alternately switched to reduce the thickness of the surface copper electroplated on the surface of the glass-based package substrate. The details are as follows:

[0075] The first stage: forward current electroplating, current density is 1ASf, time is 10min;

[0076] The second stage: forward current electroplating, current density is 2ASf, time is 40min;

[0077] The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100ms, the forward and reverse pulse time ratio is 4:1, and the total electroplating time of the third stage current is 40min;

[0078] The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 75ms, the forward and reverse pulse time ratio is 1.5:1, and the total electroplating time of the fourth stage current is 90min;

[0079] The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50ms, the forward and reverse pulse time ratio is 1:2, and the total electroplating time of the fifth stage current is 50min;

[0080] The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20ms, the forward and reverse pulse time ratio is 1:2, and the total electroplating time of the sixth stage current is 70min;

[0081] The plating solution used in electroplating includes a solution containing copper ions and other organic additives.

[0082] Example 3

[0083] In this embodiment, the glass substrate has a thickness of 510 μm, a minimum aperture of 50 μm, and an aspect ratio of about 10:1. The method for controlling the surface copper thickness during the electroplating hole filling process includes the following steps:

[0084] (1) forming a through hole on a glass-based packaging substrate;

[0085] (2) Vacuum sputtering: A layer of copper or copper alloy is plated on the surface of the glass-based package substrate and the surface of the hole by sputtering;

[0086] (3) Electroplating hole filling: segmented electroplating is adopted, and the electroplating process includes six stages of electroplating. From the first stage to the sixth stage, the electroplating current is direct current. From the third stage, positive and reverse pulse currents are alternately switched to reduce the thickness of the surface copper electroplated on the surface of the glass-based package substrate. The details are as follows:

[0087] The first stage: forward current electroplating, current density is 1ASf, time is 10min;

[0088] The second stage: forward current electroplating, current density is 2ASf, time is 60min;

[0089] The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 150ms, the forward and reverse pulse time ratio is 3:1, and the total electroplating time of the third stage current is 80min;

[0090] The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 80ms, the forward and reverse pulse time ratio is 2:1, and the total electroplating time of the fourth stage current is 110min;

[0091] The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30ms, the forward and reverse pulse time ratio is 1:1.5, and the total electroplating time of the fifth stage current is 60min;

[0092] The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30ms, the forward and reverse pulse time ratio is 1:2, and the total electroplating time of the sixth stage current is 95min.

[0093] The plating solution used in electroplating includes a solution containing copper ions and other organic additives.

[0094] Example 4

[0095] In this embodiment, the glass substrate has a thickness of 600 μm, a minimum aperture of 40 μm, and an aspect ratio of 15:1. The method for controlling the surface copper thickness during the electroplating hole filling process includes the following steps:

[0096] (1) forming a through hole on a glass-based packaging substrate;

[0097] (2) Vacuum sputtering: A layer of copper or copper alloy is plated on the surface of the glass-based package substrate and the surface of the hole by sputtering;

[0098] (3) Electroplating hole filling: Segmented electroplating is adopted, and the electroplating process includes seven stages of electroplating. From the first stage to the seventh stage, the electroplating current is direct current. From the third stage, positive and reverse pulse currents are alternately switched to reduce the thickness of the surface copper electroplated on the surface of the glass-based package substrate. The details are as follows:

[0099] The first stage: forward current electroplating, current density is 1ASf, time is 10min;

[0100] The second stage: forward current electroplating, current density is 2ASf, time is 45min;

[0101] The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100ms, the forward and reverse pulse time ratio is 4:1, and the total electroplating time of the third stage current is 100min;

[0102] The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100ms, the forward and reverse pulse time ratio is 2:1, and the total electroplating time of the fourth stage current is 150min;

[0103] The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30ms, the forward and reverse pulse time ratio is 1.5:1, and the total electroplating time of the fifth stage current is 15min;

[0104] The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20ms, the forward and reverse pulse time ratio is 1:2, and the total electroplating time of the sixth stage current is 100min;

[0105] The seventh stage: the current density is 4ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20ms, the forward and reverse pulse time ratio is 1:2, and the total electroplating time of the seventh stage current is 60min;

[0106] The plating solution used in electroplating includes a solution containing copper ions and other organic additives.

[0107] In Examples 1 to 4, step (1), forming a through hole on a glass-based packaging carrier can be accomplished by laser-induced modification and acid etching, and the specific steps are as follows: a pulsed laser beam is focused into a laser beam focal line and irradiated onto a glass substrate, the laser beam focal line generates induced absorption within the glass substrate, so that the laser beam focal line generates a defect line extending through the thickness of the glass substrate at the irradiated position, and the glass substrate irradiated with the laser beam is placed in a hydrofluoric acid solution to etch a hole, thereby avoiding cracks caused by laser peeling.

[0108] In Example 1 to Example 4, the vacuum sputtering of step (2) can be performed using a pulse power supply, the operating voltage is between 400 volts and 700 volts, and the thickness of the copper or copper alloy sputtered on the glass surface and the hole surface is 400-800nm. Due to the conductivity of the metal, sputtering copper or copper alloy on the surface of the glass-based packaging carrier and the hole surface is to facilitate the subsequent electroplating deposition step. Since the glass surface is smooth and has poor adhesion to copper, it is easy to cause stratification between the glass substrate and the metal layer, resulting in curling or even falling off of the metal layer. As a preferred embodiment, the alloy of copper, nickel and zinc is sputtered on the glass surface and the hole surface, wherein the mass fraction of copper is 75-80%, the mass fraction of nickel is 15-21%, and the mass fraction of zinc is 2-5%. Compared with copper plating, the copper alloy (copper, nickel and zinc alloy) of the present invention can improve adhesion, enhance electroplating effect, facilitate copper ion deposition in the hole, and reduce the occurrence of curling or even falling off of the electroplated metal layer. The results show that when the sputtered copper alloy is an alloy of copper, nickel and zinc, the mass fraction of copper is 79%, the mass fraction of nickel is 18% and the mass fraction of zinc is 3%, the effect is optimal, which can effectively reduce the curling of the electroplated metal layer and is not easy to fall off.

[0109] In Examples 1 to 4, during the first and second electroplating stages, a mobile spray plate or cathode plate is reciprocated to effectively ensure uniform ion concentration distribution at various locations within the TGV hole, reduce the effective thickness of the diffusion layer, and thereby improve copper deposition efficiency.

[0110] In Example 1 to Example 4, the electroplating temperature is 20 to 30° C. In the electroplating solution, the solution containing copper ions can be a copper sulfate solution; the organic additive can include a thiadiazole amide compound or a polyquaternary ammonium salt compound with a molecular weight greater than 3000, preferably a polyquaternary ammonium salt compound with a molecular weight greater than 3000. The polyquaternary ammonium salt compound is preferably a reaction product of an ether containing a tertiary amine structure and tetrachloromethylmethane alternately copolymerized, for example, it can be a reaction product of di[2-(N,N-dimethylaminoethyl)]ether and tetrachloromethylmethane, and the polyquaternary ammonium salt dosage is 50 to 150 mg / L for the best effect. Since the polyquaternary ammonium salt of the present invention is an alternating copolymer of an ether containing a tertiary amine structure and tetrachloromethylmethane, it contains a highly branched dendritic structure and has good water solubility, and since the macromolecular polymer is relatively difficult to enter the pores, the number of complexed copper ions in the pores is relatively small, thereby increasing the copper plating speed in the pores, which is beneficial to the growth of the pore copper and the control of the surface copper thickness, and the deep plating effect is good. In addition, the leveling agent of the above-mentioned polyquaternary ammonium salt can improve the dispersibility and covering power of the plating solution. Since the amine-containing functional group carries a positive charge, it is easy to be adsorbed on the high current density area, especially the area where the plate surface is protruding (the place where the copper thickness is thicker), so the copper deposition at these parts can be reduced, making the coating surface more uniform, and also helping to make the coating more compact. At this time, in combination with the segmented electroplating method of the present invention, the surface copper can be controlled to thicken and make the surface copper more flat and uniform, while being conducive to the growth of the hole copper. When the hole copper is filled, the surface copper thickness can be controlled to be thinner and is not easy to fall off. The organic additive can also include an accelerator, or include an accelerator and a wetting agent. As a preferred embodiment, the wetting agent is a polymer compound containing an ether bond, or ethylene oxide and propylene oxide are homopolymerized block copolymers.

[0111] In the embodiment 1 to the embodiment 4 of the present invention, the electroplating process includes six or seven electroplating current sections. The present invention can save electroplating time, improve electroplating efficiency, and effectively control the surface copper thickness while filling the hole. In addition, the current density used in the electroplating process of the present invention is relatively small as a whole, which can help make the copper more compact. Among them, the electroplating current density of the first section is small. In the first section of the electroplating process, there is basically no copper deposition on the plate surface of the hole and the glass substrate. The main function of the first section of the electroplating is to discharge the bubbles (hydrogen) in the hole by vibration, and at the same time, the surface of the glass substrate and the through hole are soaked and wetted by the jet, so as to facilitate the subsequent electroplating reaction and the deposition of copper. Starting from the second section of the electroplating, copper is gradually deposited on the plate surface of the hole and the glass substrate. The second section of the electroplating is only the forward current electroplating, which can save electroplating time, improve electroplating efficiency, and is conducive to the rapid growth of hole copper. When the hole copper is deposited to a certain extent, the surface copper has also been deposited to a certain thickness. By continuously switching the current direction, under the action of the reverse pulse current, the surface copper will be dissolved, thereby making the surface copper thinner. The copper on the surface of the hole mouth may also be partially dissolved during the reverse current, but because the hole is a low current density area, and the reverse current is a pulse current with a shorter time (it will soon switch to a forward current), the copper in the hole will continue to be deposited and will hardly be dissolved. Therefore, the present invention can ensure that the copper in the hole is getting thicker and thicker while thinning the surface copper. Usually, in the entire electroplating process, the total time of the fourth section electroplating is the longest. At the end of the fourth section electroplating set by the present invention, the copper in the hole is about to be filled or has been basically filled and filled. The main function of the fifth to seventh sections of electroplating is to thin the thickness of the surface copper and make the copper in the hole continue to fill and fill. The present invention uses multi-segment pulse electroplating to reasonably design the forward and reverse current density and time, so that the copper layer in the hole becomes thicker and thicker, making it difficult to fall off, and at the same time, the surface copper can be made thinner and thinner, reducing the thickness of the surface copper, which is beneficial to the subsequent fine circuit production.

[0112] The effect of the surface copper thickness control method in the electroplating hole filling process of the present invention is verified by using electroplating solution A and electroplating solution B respectively, and verification examples are set, namely, Examples 5 to 7, wherein Example 5 is a comparative example, electroplating solution A is a commonly used electroplating solution formula in the prior art, and electroplating solution B is a leveling agent containing the above-mentioned polyquaternary ammonium salt of the present invention. The formulas of electroplating solution A and electroplating solution B are as follows:

[0113] Plating solution A: the leveling agent is denazur green, the dosage is 6 mg / L; copper sulfate pentahydrate 220 g / L, sulfuric acid (98%) 60 g / L, chloride ion 36 mg / L, sodium polydisulfide bis(propylene sulfonate) (SPS) 6 mg / L, PEG (polyethylene glycol) 600 mg / L.

[0114] Plating solution B: polyquaternium salt leveler 100 mg / L; copper sulfate pentahydrate 220 g / L, sulfuric acid (98%) 60 g / L, ferrous chloride 85 mg / L, sodium polydisulfide propane sulfonate (SPS) 20 mg / L, PEG (polyethylene glycol) 300 mg / L. The preparation method of the polyquaternary ammonium salt leveler is as follows: 21g (i.e. 0.1mol) of tetrachloromethylmethane, 32g (i.e. 0.2mol) of di[2-(N,N-dimethylaminoethyl)]ether and 180ml of anhydrous ethanol are weighed respectively, and the weighed tetrachloromethylmethane, di[2-(N,N-dimethylaminoethyl)]ether and anhydrous ethanol are poured into a reaction container, stirred evenly at room temperature, and heated to 60°C under the protection of an inert gas (such as nitrogen), and kept at a constant temperature for 18h, cooled, and ethanol was removed under reduced pressure. After recrystallization, the polyquaternary ammonium salt leveler: polytetrachloromethylmethane-di[2-(N,N-dimethylaminoethyl)]ether quaternary ammonium salt is obtained.

[0115] Example 5

[0116] This embodiment is a comparative example. Electroplating solution A is used to electroplating and filling holes in the TGV to be plated. The thickness of the glass substrate to be plated is about 425 μm, the minimum hole diameter is about 70 μm, and the aspect ratio is about 6:1. Before electroplating, the substrate to be plated is pre-metallized on the plate surface and in the hole; the electroplating current density is 1.5 A / dm 2 , the electroplating temperature is 25°C, air stirring, and the electroplating time is 90 minutes. The surface copper thickness of the conventional electroplating method in the prior art is usually thicker (such as Figure 2 , the surface copper thickness is usually more than 30μm), and it is very easy to have holes (such as Figure 3 ).

[0117] Example 6

[0118] In this embodiment, electroplating solution A is used to electroplate and fill holes in the TGV to be plated. The thickness of the glass substrate to be plated is about 425 μm, the minimum pore size is about 70 μm, and the aspect ratio is about 6:1. The electroplating method and steps are the same as those in Example 2 of the present invention. The electroplating results are as follows: Figure 4 shown.

[0119] Example 7

[0120] In this embodiment, electroplating solution B is used to electroplate and fill holes in the TGV to be plated. The plate thickness to be plated is 388.2 μm, the minimum pore size is 92.6 μm, and the aspect ratio is about 4.2:1. The electroplating method and steps are the same as those in Example 1 of the present invention. The electroplating results are as follows: Figure 5 shown.

[0121] Depend on Figure 2-Figure 5It can be seen that the electroplating hole filling method of the present invention can effectively control the surface copper thickness compared with the prior art, which can generally be controlled within 14 μm, and can even be controlled within 2-5 μm (such as Figure 5 , i.e., Example 7, in which the surface copper thickness is only 2.4-4.1 μm), significantly reducing the surface copper thickness.

[0122] The above description is only an example of the present invention and is not intended to limit the present invention in other forms. Any technician familiar with the profession may use the technical contents disclosed above to change or modify them into equivalent embodiments with equivalent changes and apply them to other fields. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the technical solution content of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for controlling the copper thickness of a glass-based package substrate electroplating hole filling surface, comprising the following steps: (1) forming a through hole on a glass-based packaging substrate; (2) Vacuum sputtering: A layer of copper or copper alloy is plated on the surface of the glass-based package substrate and the surface of the hole by sputtering; (3) Electroplating hole filling: segmented electroplating is adopted, and the electroplating current is direct current. From the third segment, positive and reverse pulse currents are alternately switched to reduce the thickness of the surface copper plated on the surface of the glass-based package substrate. The details are as follows: The first stage: forward current electroplating, current density is 1ASf, time is 10~15min; The second stage: forward current electroplating, current density is 2ASf, time is 30~60min; The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100-150ms, the forward and reverse pulse time ratio is (2:1)-(4:1), and the total electroplating time of the third stage current is 5-120min; The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50 to 100ms, the forward and reverse pulse time ratio is (1:1) to (2:1), and the total electroplating time of the fourth stage current is 60 to 180min; The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30 to 50ms, the forward and reverse pulse time ratio is (1:2) to (2:1), and the total electroplating time of the fifth stage current is 10 to 120min; The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20 to 30ms, the forward and reverse pulse time ratio is (1:1) to (1:3), and the total electroplating time of the sixth stage current is 60 to 120min; The seventh stage: the current density is 3-5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20-30ms, the forward and reverse pulse time ratio is (1:1)-(1:3), and the total electroplating time of the seventh stage current is greater than or equal to 0min and less than or equal to 60min; The plating solution used in electroplating includes a solution containing copper ions and other organic additives.

2. The method for controlling the copper thickness of the via-filling surface of the glass-based package substrate electroplating according to claim 1, It is characterized in that The specific steps of step (3) of segmented electroplating and hole filling are as follows: The first stage: forward current electroplating, current density is 1ASf, time is 10min; The second stage: forward current electroplating, current density is 2ASf, time is 30~50min; The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100-150ms, the forward and reverse pulse time ratio is (2:1)-(4:1), and the total electroplating time of the third stage current is 5-60min; The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50 to 100ms, the forward and reverse pulse time ratio is (1:1) to (2:1), and the total electroplating time of the fourth stage current is 60 to 90min; The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30 to 50ms, the forward and reverse pulse time ratio is (1:1) to (1:2), and the total electroplating time of the fifth stage current is 20 to 80min; The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20 to 30ms, the forward and reverse pulse time ratio is (1:1) to (1:2), and the total electroplating time of the sixth stage current is 60 to 80min.

3. The method for controlling the copper thickness of the via-filling surface of the glass-based package substrate electroplating according to claim 1, It is characterized in that The specific steps of step (3) of segmented electroplating and hole filling are as follows: The first stage: forward current electroplating, current density is 1ASf, time is 10min; The second stage: forward current electroplating, current density is 2ASf, time is 50-60min; The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100-150ms, the forward and reverse pulse time ratio is (2:1)-(4:1), and the total electroplating time of the third stage current is 70-100min; The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50 to 100ms, the forward and reverse pulse time ratio is (1:1) to (2:1), and the total electroplating time of the fourth stage current is 100 to 150min; The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30 to 50ms, the forward and reverse pulse time ratio is (1:1) to (1:2), and the total electroplating time of the fifth stage current is 60 to 120min; The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20 to 30ms, the forward and reverse pulse time ratio is (1:1) to (1:3), and the total electroplating time of the sixth stage current is 90 to 120min.

4. The method for controlling the copper thickness of the via-filling surface of the glass-based package substrate electroplating according to claim 1, It is characterized in that The specific steps of step (3) of segmented electroplating and hole filling are as follows: The first stage: forward current electroplating, current density is 1ASf, time is 10min; The second stage: forward current electroplating, current density is 2ASf, time is 40~60min; The third stage: the current density is 3ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 100-150ms, the forward and reverse pulse time ratio is (2:1)-(4:1), and the total electroplating time of the third stage current is 100-120min; The fourth stage: the current density is 5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 50 to 100ms, the forward and reverse pulse time ratio is (1:1) to (2:1), and the total electroplating time of the fourth stage current is 130 to 180min; The fifth stage: the current density is 7ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 30 to 50ms, the forward and reverse pulse time ratio is (1:2) to (2:1), and the total electroplating time of the fifth stage current is 10 to 80min; The sixth stage: the current density is 9ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20 to 30ms, the forward and reverse pulse time ratio is (1:1) to (1:2), and the total electroplating time of the sixth stage current is 80 to 120min; The seventh stage: the current density is 3-5ASf, the forward current and the reverse current are switched alternately, the forward pulse time is 20-30ms, the forward and reverse pulse time ratio is (1:1)-(1:3), and the total electroplating time of the seventh stage current is 40-60min.

5. The method for controlling the copper thickness of the via-filling surface of the glass-based package substrate electroplating according to claim 1, It is characterized in that During the first and second stages of electroplating, a moving spray plate or cathode plate is used to reciprocate.

6. The method for controlling the copper thickness of the via-filling surface of the glass-based package substrate electroplating according to claim 1, It is characterized in that The sputtering is performed using a pulse power supply, and the thickness of the copper or copper alloy sputtered on the surface of the glass-based packaging carrier and the surface of the hole is 400-800nm.

7. The method for controlling the copper thickness of the via-filling surface of the glass-based package substrate electroplating according to claim 1, It is characterized in that The alloy of copper, nickel and zinc is sputtered on the glass surface and the hole surface, wherein the mass fraction of copper is 75-80%, the mass fraction of nickel is 15-21% and the mass fraction of zinc is 2-5%.

8. The method for controlling the copper thickness of the via-filling surface of the glass-based package substrate electroplating according to claim 1, It is characterized in that The solution containing copper ions is a copper sulfate solution, and the organic additive comprises a thiadiazole amide compound and / or a polyquaternary ammonium salt compound with a molecular weight greater than 3,000.

9. A glass product obtained according to the method according to any one of claims 1 to 8.

10. Application of the glass product according to claim 9 in the fields of optical communication, radio frequency, microwave, micro-electromechanical system, microfluidic device and three-dimensional integration and MEMS packaging.

Citation Information

Cited By

  • Glass adapter plate, filling method of glass through hole of glass adapter plate and chip

    CN119640351A

  • A glass adapter plate and a method of filling glass vias thereof and a chip

    CN119640351B