Preparation method of luminous artificial spider thread, luminous surgical suture and fluorescent protective net

By regulating the properties of the spinning liquid with organic acid derivatives and polyhydroxy monomers, and directly spinning the artificial spider silk with high strength and toughness and spinability is solved by directly spinning the artificial spider silk in the prior art and it is difficult to achieve high strength and toughness and The problem of stable luminescence and improves the mechanical and fluorescence properties of the fibers.

CN118996653APending Publication Date: 2024-11-22CHINA PHARM UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410969921.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to achieve high strength, spunability and stable luminescence artificial spider silk at the same time, and commonly used chromophore preparation methods are prone to cause leakage and quenching under light irradiation.

Method used

Using organic acid derivatives and polyhydroxy monomers with high hydration and aggregation-induced luminescence properties, the spinning and fluorescence properties of the spinning liquid are regulated by changing the monomer ratio and concentration, and crosslinking agent is introduced to improve the mechanical properties, directly Spinning to prepare luminescent artificial spider silk.

Benefits of technology

Artificial spider silk with high strength, toughness, good spinning and long-lasting stable luminescence were successfully prepared, and the luminous performance of the fibers was not affected after the addition of crosslinking agent. It is suitable for surgical sutures and fluorescent protective nets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996653A_ABST
    Figure CN118996653A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a luminous artificial spider thread, a luminous surgical suture and a fluorescent protective net, and relates to the field of high polymer material preparation. According to the method, an organic acid derivative with an aggregation-induced emission property and a polyhydroxy monomer are used as raw materials, under the action of an initiator, ultraviolet light polymerization is performed to obtain a spinning solution, and then direct spinning is performed to continuously prepare the luminous artificial spider silk. The mechanical property can be regulated and enhanced by adding a hydroxyl monomer, and the mechanical property can be further enhanced by introducing a cross-linking agent and twisting. The tensile strength of the luminous artificial spider silk is 506 MPa, the stretchability is 24%, the fluorescence quantum yield is 15.6%, and the luminous artificial spider silk is high in light stability and not prone to being bleached. The strategy of preparing the fiber by combining aggregation-induced emission with a plurality of hydrogen bond fragments can also excite new designs in the aspects of 3D printing, advanced infrastructure and buildings, and the spinning method taking spiders as inspiration is an environment-friendly and energy-saving method, and can reduce the release of carbon in the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polymer material preparation, and particularly relates to a method for preparing luminous artificial spider silk. Background Art

[0002] In nature, spiders continuously spin fibers from protein spinning solutions under ambient conditions. The multi-level structure of spider silk and its unique spinning process are key factors in achieving its excellent properties. During the spider spinning process, the protein peptide chains of the spinning solution in the S-tubes are highly hydrated, so they can change their morphology under shear stress and become highly spinnable. Subsequently, multiple hydrogen bonds are formed in the β-sheets and amorphous regions, which contribute to the strength and toughness of spider silk. In addition, jellyfish can exhibit aggregation-induced luminescence, which is achieved by the self-assembly of hydrated functional groups in a confined space without the use of common conjugated chromophores, and the luminescence of jellyfish has the characteristics of long life and small attenuation. Therefore, it is of great significance in real life to imitate spider spinning, spider silk structure and jellyfish luminescence mechanism to develop artificial spider silk with good spinnability, high strength and toughness, and long-term stable luminescence, and apply it to fields such as shock absorption and energy absorption, such as life preservers for humans or moving cars, and protective nets for damping the impact of high-speed objects in the dark.

[0003] At present, different types of strong polymer artificial spider silk have been prepared by mimicking the structure of spider silk, including protein-like nanogels, artificial spider silk with a buckled sheath-core structure combed by nanopulleys, neuronal ionomers for signal transmission, pseudoprotein polymers by introducing β-folds and α-helices, supramolecular elastomers with geometrically restricted hydrogen bond arrays, polyaniline fibers spun by solvent exchange, and dry-spinning nematic silk from microfiber stock solutions. However, it is still challenging to develop artificial spider silk with spinnability, high strength and toughness, and stable luminescence. In the past, the preparation of luminescent fibers by adding chromophores may cause leakage, and the chromophores are easily quenched under light irradiation. Therefore, it is urgent to spin strong and tough artificial spider silk with high luminescence by adopting molecular engineering to simultaneously achieve high hydration, adjustable hydrogen bonding, and aggregation-induced light emission. Summary of the invention

[0004] The purpose of the present invention is to enrich the spinning system of artificial spider silk, how to improve the spinnability and mechanical properties of artificial spider silk, and to provide a method for preparing luminous artificial spider silk for use in special application scenarios. At the same time, a method for preparing luminous surgical sutures and fluorescent protective nets is further provided.

[0005] The technical solution of the present invention is:

[0006] The present invention starts from the mechanism of spider spinning, spider silk structure and jellyfish luminescence, introduces organic acid derivatives with high hydration and aggregation-induced luminescence properties and polyhydroxy monomers that can form multiple hydrogen bonds to polymerize and prepare spinning solution, and directly spins to prepare luminous artificial spider silk. The spinnability, toughness and fluorescence properties of artificial spider silk are regulated by changing the ratio and concentration of monomers, and the mechanical properties are further improved by introducing crosslinking agents and twisting, and the long-lasting and stable luminescence of the fiber will not be affected.

[0007] A method for preparing luminous artificial spider silk comprises the following steps:

[0008] Step 1: dissolving an organic acid derivative and a polyhydroxy monomer in deionized water, adding a crosslinking agent and an initiator, and stirring to obtain a prepolymer solution;

[0009] Step 2: Blowing an inert gas into the prepolymer solution in step 1 to obtain a spinning solution through free radical polymerization;

[0010] Step 3: Directly spin the spinning solution in step 2 to obtain luminous artificial spider silk or hydrogel fiber.

[0011] The organic acid derivative can be replaced by one of 2-acrylamide-2-methylpropanesulfonic acid, acrylic acid, acrylamide, methacrylic acid, propylene sulfonic acid, cis-acrylphosphoric acid, N-acryloylglycine, N-acryloylalanine, N-acryloylbutyric acid, and N-(2-amino-2-oxoethyl)acrylamide.

[0012] The polyhydroxy monomer is one of the following: N-hydroxyethyl acrylamide, N-dihydroxymethyl methacrylamide, N-trihydroxymethyl methacrylamide, polyvinyl alcohol.

[0013] The initiator can be replaced by one of ammonium persulfate, potassium persulfate, 2-hydroxy-2-methyl-1-phenylacetone and α-ketoglutaric acid, accounting for 0.1-0.5 mol% of the total monomers.

[0014] The cross-linking agent is N,N'-methylenebisacrylamide (MBAA), accounting for 0-0.05 mol% of the total monomers.

[0015] The inert gas blown in step 2 may be one of nitrogen and argon, and the blowing time is 1-10 min.

[0016] In step 2, the prepolymer solution is injected into a tubular mold such as a glass capillary for polymerization.

[0017] The initiation condition of the free radical polymerization in step 2 may be one of heating polymerization and ultraviolet polymerization.

[0018] Preferably, the conditions for the heating polymerization are as follows: the prepolymer solution is heated at a temperature of 40-60° C. for 1-12 hours.

[0019] Preferably, the conditions for UV polymerization are as follows: the prepolymer solution is polymerized under UV light with a power of 8-20 W for 0.5-6 hours.

[0020] The spinning method in step 3 can be one of the following: breaking off a tubular mold such as a glass capillary and directly stretching and spinning, using an iron rod dipped in spinning solution to directly stretch and spin, or dry spinning.

[0021] The spinning in step 3 can obtain fibers with a diameter of 5-300 microns.

[0022] The shaping time of the luminous artificial spider silk in step 3 is 30-300 seconds.

[0023] The drying condition of the luminous artificial spider silk in step 3 is 30-100° C. for 1-15 hours.

[0024] Furthermore, the present invention provides a luminous surgical suture, which comprises an inner core and a coating, and comprises the following steps:

[0025] The hydrogel fiber obtained by the above method is used as an inner core to penetrate into the coating solution, and then taken out and dried to obtain a luminous surgical suture;

[0026] The coating solution includes cellulose triacetate (CTA), sodium alginate (SA), polylactic acid (PLA), sodium alginate / chitosan (SA / CS), sodium alginate / Ca 2+ (SA / Ca 2+ ), any one of the solutions of polymethyl acrylate (PMA), polyvinyl alcohol 1799 (PVA1799), gelatin / chitosan / phytate (GEL / CS / SP); the time for the inner core hydrogel fiber to invade the coating solution is 3-10 seconds; the inner core hydrogel fiber is taken out from the coating solution and dried for 1-12 hours.

[0027] The diameter of the inner core hydrogel fiber is 50-220 μm, and the thickness of the coating is 10-30 μm.

[0028] Furthermore, the present invention provides a method for preparing a fluorescent protection net, comprising the following steps:

[0029] Step 1: Twisting the hydrogel fibers obtained by the above method into fluorescent yarns;

[0030] Step 2: Weaving the fluorescent yarn obtained in step 1 into a fluorescent protective net according to a certain fabric density;

[0031] The fluorescent protection net woven according to a certain fabric density refers to: the warp density is 1 yarn per inch, the weft density is 2 yarns per inch, the warp length is 15 cm, and the weft length is 20 cm.

[0032] Advantages and beneficial effects of the present invention:

[0033] 1. The present invention proposes a strategy for preparing luminous artificial spider silk fibers, which has the advantages of readily available raw materials, low cost, environmental friendliness and simple preparation.

[0034] 2. The present invention achieves the regulation of the spinnability, mechanical properties and fluorescence properties of the luminescent artificial spider silk by changing the concentration and ratio of the organic acid derivatives and the polyhydroxy monomers, and successfully prepares the artificial spider silk with high strength, good spinnability and long-lasting and stable luminescence.

[0035] 3. After adding 0.01% MBAA crosslinking agent and introducing 9 turns / cm, the luminous artificial spider silk prepared by the present invention is dried at 60°C for 9 hours to achieve a breaking strength of 506 MPa and a breaking toughness of 108 MJ / m 3 And after irradiation with 365nm ultraviolet light for 60h, the fluorescence intensity of the fiber hardly decayed.

[0036] 4. In the preparation method of surgical sutures of the present invention, the fiber is immersed in the coating solution for a certain period of time by a dipping method. After the luminous fiber is taken out, the solvent evaporates quickly so that the coating can easily form a film on the surface of the suture. The fiber and the film are combined with each other to protect the internal suture from external influences and improve the smoothness of the suture surface, so that the mechanical properties of the luminous surgical suture with an inner core and a coating structure are greatly improved, and the luminous performance is not affected, thereby improving the safety and stability of the surgical suture during actual use.

[0037] 5. The preparation method of the luminous surgical suture of the present invention uses direct stretch spinning and dip coating to produce a surgical suture with excellent mechanical properties and long-lasting luminescence. Moreover, by means of coating, the mechanical properties of the fiber are improved while the water resistance of the fiber is also improved, providing a new strategy for preparing water-resistant fiber materials. In addition, the preparation method is simple and convenient, and the obtained luminous surgical suture has good mechanical properties, water resistance, and good biocompatibility, meeting clinical needs.

[0038] 6. The fluorescent protection net and its preparation method proposed in the present invention have the advantages of easy availability of raw materials, low cost, environmental friendliness and simple preparation. The yarn density and fabric density can be adjusted as needed to prepare the fluorescent protection net, achieving customizability.

[0039] 7. The fluorescent protective net prepared by the present invention can be used as a life-saving device for objects moving at high speed in weak light and dark scenes. It is expected to be used in protective nets for roads, railways and airports, isolation nets to prevent falling rocks and falling objects, and aerospace fields, and has broad application fields and prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 A synthetic route for luminescent artificial spider silk.

[0041] Figure 2 These are metallographic fiberscope and fluorescence photographs of luminous artificial spider silk.

[0042] Figure 3 (a) is a graph showing the mechanical properties test results of fibers containing different numbers of hydroxyl groups; (b) is a graph showing the fluorescence quantum yield test results of fibers containing different numbers of hydroxyl groups.

[0043] Figure 4 (a) is the stress-strain curve of the hydrogel fiber containing different monomer molar ratios; (b) is the fluorescence quantum yield test result of the hydrogel fiber containing different monomer molar ratios.

[0044] Figure 5 This is a graph showing the mechanical properties test results of hydrogel fibers containing different mole fractions of cross-linking agents.

[0045] Figure 6 Figure 2 shows the mechanical properties test results of hydrogel fibers with different twist densities.

[0046] Figure 7 (a) is a graph showing the mechanical properties test results of the hydrogel fiber dried at 40°C for different times; (b) is a graph showing the mechanical properties test results of the hydrogel fiber dried at different temperatures for 9 hours.

[0047] Figure 8 This is a graph showing the mechanical properties test results of hydrogel fibers at different tensile speeds.

[0048] Fig. 9 This is a picture of the fluorescent fiber artificial muscle contracting under water mist stimulation.

[0049] Fig.10 The graph shows the contraction rate and work results of artificial muscles containing different numbers of hydroxyl groups.

[0050] Fig.11 The driving percentage and working capacity of the fiber under different loads.

[0051] Fig.12 The maximum working capacity of different fibers.

[0052] Fig.13 Schematic diagram of the preparation of luminous surgical sutures.

[0053] Fig.14 is the swelling ratio of uncoated and coated fibers.

[0054] Fig.15 The figures show the mechanical properties and water resistance results of uncoated and coated fibers.

[0055] Fig.16 Fluorescence images of uncoated and coated fibers.

[0056] Fig.17 The graph shows the cytotoxic activity results of uncoated and polylactic acid coated fibers.

[0057] Fig.18 (a) is the damping capacity of the fluorescent hydrogel fiber; (b) is the "loading-unloading" test diagram of the fluorescent hydrogel fiber.

[0058] Fig.19 The damping capacity and stress results of fluorescent hydrogel fibers after cyclic loading and unloading. After each cycle, the fibers shrink to their original length under high humidity.

[0059] Fig. 20 (a) Supercontraction of fluorescent hydrogel fibers at 65% relative humidity; (b) The degree of shrinkage during a cyclic test between relative humidity of 25% and 65%, where the fluorescent hydrogel fibers recovered their initial length after the supercontraction period.

[0060] Fig.21 The fluorescent protective net stopped a 240g toy airplane moving at 90cm / s under a relative humidity of 60%, and the huge deformation returned to its original shape.

[0061] Fig. 22 The images of intact and broken fluorescent surgical sutures under the mouse skin under 365nm and daylight. The arrow indicates the location of the fluorescent surgical suture, and the dotted circle indicates the location where the fluorescent surgical suture is broken. DETAILED DESCRIPTION

[0062] Embodiment 1:

[0063] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is described in detail below with reference to the accompanying drawings.

[0064] The method for preparing luminous artificial spider silk comprises the following steps:

[0065] Step 1: dissolving 2-acrylamide-2-methylpropane sulfonic acid and polyhydroxy monomer in 1 ml of deionized water, wherein the molar ratio of polyhydroxy monomer to 2-acrylamide-2-methylpropane sulfonic acid is 0-3, and the total monomer concentration is 1.0-3.8 mol / l, adding 0.068 mg of ammonium persulfate, and stirring to obtain a prepolymer solution;

[0066] Step 2: After nitrogen is bubbled into the prepolymer solution of step 1 for 3-5 minutes, the prepolymer solution is injected into a glass capillary with an inner diameter of 0.1-1.0 mm, and 254 nm ultraviolet light with a power of 8 W is used for 4 hours to obtain a spinning solution;

[0067] Step 3: Break the glass capillary in step 2, and directly stretch and spin to obtain luminous artificial spider silk;

[0068] Step 4: Fix the two ends of the luminous artificial spider silk obtained in step 3 on the rack and dry it to shape.

[0069] Figure 1 The synthetic route for luminescent hydrogel fibers.

[0070] Figure 2 These are metallographic microscope and fluorescence photographs of artificial spider silk.

[0071] The luminous artificial spider silk fiber finally obtained in this example was subjected to the following tests:

[0072] Mechanical property test: The luminous artificial spider silk with a diameter of 120 microns and containing different hydroxyl monomers was subjected to tensile test (tensile rate of 20 mm / min) under the condition of 25% air humidity. Figure 3 As shown in (a), this figure illustrates that as the number of hydroxyl groups increases, the breaking strength of the luminous artificial spider silk increases and the breaking strain increases.

[0073] Fluorescence quantum yield test: the luminescent artificial spider silk with a diameter of 120 microns and containing different hydroxyl monomers was dried for 24 hours under the condition of air humidity of 25%, and then the fluorescence quantum yield test was carried out. Figure 3 (b) shows that the fluorescence quantum yield of the luminescent artificial spider silk increases with the increase of the number of hydroxyl groups.

[0074] Embodiment 2:

[0075] The method for preparing luminous artificial spider silk comprises the following steps:

[0076] Step 1: dissolving 2-acrylamide-2-methylpropanesulfonic acid and N-trimethylolmethyl acrylamide in 1 ml of deionized water, wherein the molar ratio of N-trimethylolmethyl acrylamide to 2-acrylamide-2-methylpropanesulfonic acid is 0-0.5, and the total monomer concentration is 1.0-3.8 mol / l, adding 0.068 mg of ammonium persulfate, and stirring to obtain a prepolymer solution;

[0077] Step 2: After nitrogen is bubbled into the prepolymer solution of step 1 for 3-5 minutes, the prepolymer solution is injected into a glass capillary with an inner diameter of 0.1-1.0 mm, and 254 nm ultraviolet light with a power of 8 W is used for 4 hours to obtain a spinning solution;

[0078] Step 3: Break the glass capillary in step 2, and directly stretch and spin to obtain luminous artificial spider silk;

[0079] Step 4: Fix the two ends of the luminous artificial spider silk obtained in step 3 on the rack and dry it to shape.

[0080] The luminous artificial spider silk fiber finally obtained in this example was subjected to the following tests:

[0081] Mechanical property test: luminous artificial spider silk with a diameter of 120 microns and containing different monomer molar ratios was subjected to tensile test (tensile rate of 20 mm / min) under the condition of air humidity of 25%. Figure 4 As shown in (a), this figure illustrates that as the molar ratio of N-trishydroxymethyl methacrylamide to 2-acrylamide-2-methylpropanesulfonic acid increases, the breaking strength of the luminous artificial spider silk increases and the breaking strain decreases.

[0082] Fluorescence quantum yield test: the luminescent artificial spider silk with a diameter of 120 microns and containing different monomer molar ratios was dried for 24 hours under the condition of air humidity of 25% and then the fluorescence quantum yield test was performed. Figure 4 (b) shows that, as the molar ratio of N-trishydroxymethyl methacrylamide to 2-acrylamide-2-methylpropanesulfonic acid increases, the fluorescence quantum yield of the luminescent artificial spider silk increases.

[0083] Embodiment 3:

[0084] The method for preparing luminous artificial spider silk comprises the following steps:

[0085] Step 1: dissolving 2-acrylamide-2-methylpropanesulfonic acid and N-trimethylolmethyl acrylamide in 1 ml of deionized water, wherein the molar ratio of N-trimethylolmethyl acrylamide to 2-acrylamide-2-methylpropanesulfonic acid is 0.5, and the total monomer concentration is 3.0-3.8 mol / l, and then adding 0.1 mol% of ammonium persulfate, stirring evenly to obtain a prepolymer solution;

[0086] Step 2: After nitrogen is bubbled into the prepolymer solution of step 1 for 3-5 minutes, the prepolymer solution is injected into a glass capillary with an inner diameter of 0.1-1.0 mm, and 254 nm ultraviolet light with a power of 8 W is used for 4 hours to obtain a spinning solution;

[0087] Step 3: Break the glass capillary in step 2, and directly stretch and spin to obtain luminous artificial spider silk;

[0088] Step 4: Fix the two ends of the luminous artificial spider silk obtained in step 3 on the rack and dry it to shape.

[0089] The luminous artificial spider silk fiber finally obtained in this example was subjected to the following tests:

[0090] Mechanical property test: luminous artificial spider silk with a diameter of 120 microns and different solid contents was subjected to tensile test (tensile rate of 20 mm / min) under the condition of air humidity of 25%. Figure 5 As shown in (a), the figure illustrates that when the total monomer concentration is 3.8 mol / l, the maximum breaking strength of the luminous artificial spider silk is 89 MPa and the breaking strain is 32%.

[0091] Embodiment 4:

[0092] The method for preparing luminous artificial spider silk comprises the following steps:

[0093] Step 1: 2-acrylamide-2-methylpropanesulfonic acid and N-trihydroxymethyl methacrylamide are dissolved in 1 ml of deionized water, wherein the molar ratio of N-trihydroxymethyl methacrylamide to 2-acrylamide-2-methylpropanesulfonic acid is 0.5, and the total monomer concentration is 3.8 mol / l, and 0, 0.005%, 0.01%, and 0.05% of MBAA are added respectively, and then 0.1 mol% of ammonium persulfate is added, and the mixture is stirred evenly to obtain a prepolymer solution;

[0094] Step 2: After nitrogen is bubbled into the prepolymer solution of step 1 for 3-5 minutes, the prepolymer solution is injected into a glass capillary with an inner diameter of 0.1-1.0 mm, and 254 nm ultraviolet light with a power of 8 W is used for 4 hours to obtain a spinning solution;

[0095] Step 3: Break the glass capillary in step 2, and directly stretch and spin to obtain luminous artificial spider silk;

[0096] Step 4: Fix the two ends of the luminous artificial spider silk obtained in step 3 on the rack and dry it to shape.

[0097] The luminous artificial spider silk fiber finally obtained in this example was subjected to the following tests:

[0098] Mechanical property test: The luminous artificial spider silk with a diameter of 120 microns and containing different mole fractions of cross-linking agent was subjected to tensile test (tensile rate of 20 mm / min) under the condition of 25% air humidity. Figure 5 As shown in (b), the figure illustrates that when MBAA accounts for 0.01% of the total monomers, the maximum breaking strength of the luminous artificial spider silk is 101 MPa and the breaking strain is 37%.

[0099] Embodiment 5:

[0100] The method for preparing luminous artificial spider silk comprises the following steps:

[0101] Step 1: dissolving 2-acrylamide-2-methylpropanesulfonic acid and N-trimethylolmethylacrylamide in 1 ml of deionized water, wherein the molar ratio of N-trimethylolmethylacrylamide to 2-acrylamide-2-methylpropanesulfonic acid is 0.5, and the total monomer concentration is 3.8 mol / l, adding 0.01% MBAA, and then adding 0.1 mol% ammonium persulfate, stirring evenly to obtain a prepolymer solution;

[0102] Step 2: After nitrogen is bubbled into the prepolymer solution of step 1 for 3-5 minutes, the prepolymer solution is injected into a glass capillary with an inner diameter of 0.1-1.0 mm, and 254 nm ultraviolet light with a power of 8 W is used for 4 hours to obtain a spinning solution;

[0103] Step 3: Break the glass capillary in step 2, and directly stretch and spin to obtain luminous artificial spider silk;

[0104] Step 4: Fix the two ends of the fiber obtained in step 3 on a rack, dry and shape it, and finally obtain luminous artificial spider silk;

[0105] Step 5: Fix one end of the luminous artificial spider silk obtained in step 4 on the motor, hang a small weight on the other end, and twist it. The twisting density is 0, 3, 6, 9, 12, and 15 turns / cm respectively;

[0106] Step 6: The luminescent artificial spider silk obtained in step 5 was dried at different temperatures for different times and tested for tensile mechanical properties using different tensile speeds (20 mm / min, 60 mm / min, 100 mm / min and 140 mm / min).

[0107] The artificial spider silk fiber finally obtained in this embodiment was subjected to the following tests:

[0108] Mechanical property test: luminous artificial spider silk with a diameter of 20 microns and different twisting densities was subjected to tensile test (tensile rate of 20 mm / min) under the condition of air humidity of 25%. Figure 6As shown in the figure, when the twisting density is 9 turns / cm, the breaking strength of the luminous artificial spider silk is 354 MPa at most, and the breaking strain is 32%.

[0109] Mechanical property test: The luminous artificial spider silk with a diameter of 20 microns and a twist density of 9 turns / cm was dried at 40°C for different times and subjected to tensile test (tensile rate of 20 mm / min). Figure 7 As shown in (a), the figure illustrates that when dried for 9 hours, the maximum breaking strength of the luminous artificial spider silk is 427 MPa and the breaking strain is 30%.

[0110] Mechanical property test: The luminous artificial spider silk with a diameter of 20 microns and a twist density of 9 turns / cm was dried at different temperatures for 9 hours and subjected to tensile test (tensile rate of 20 mm / min). Figure 7 As shown in (b), the figure illustrates that when the temperature is 60°C, the maximum breaking strength of the luminous artificial spider silk is 478 MPa and the breaking strain is 28%.

[0111] Mechanical property test: The luminous artificial spider silk with a diameter of 20 μm and a twist density of 9 turns / cm was dried at 60 °C for 9 h and tested at different tensile speeds (20 mm / min, 60 mm / min, 100 mm / min and 140 mm / min). Figure 8 As shown in the figure, when the tensile speed is 140 mm / min, the maximum breaking strength of the luminous artificial spider silk is 506 MPa, and the breaking strain is 24%.

[0112] Jellyfish emit fluorescence through the self-assembly of hydrated functional groups in a confined space without the use of common conjugated chromophores, and the luminescence of jellyfish has the characteristics of long life and small attenuation under external excitation. In addition, in a high humidity environment, the length of spider silk will shrink sharply by about 50%. This process is usually called supercontraction. This property not only plays a good protective role for spider silk, but also makes it have potential application value in the field of artificial muscles or stretch actuators. Artificial muscle is a new type of bionic flexible actuator, similar to biological muscle, with the characteristics of large contraction stress, high power density and high energy conversion efficiency. In particular, fiber artificial muscles are widely used in sensors, controllers, tissue engineering, health care, soft robots and other fields due to their simple structure, light weight and low cost.

[0113] Artificial muscles can be actuated by a variety of driving methods. Compared with other stimulation media, water is cheap, easy to supply, environmentally friendly and non-toxic, so it is increasingly favored as a medium for driving artificial muscles. Most of the fiber-type artificial muscles reported so far increase their driving stroke through twisting technology, but they cannot be widely used due to their complex structure or lack of universality. In addition, the philtrum muscle that can be used in multiple scenarios by utilizing its own luminous characteristics has not yet been developed. Therefore, the field of fiber artificial muscle technology urgently needs to prepare a new type of luminous fiber artificial muscle to increase the function of existing fiber artificial muscles, so as to promote the application of fiber artificial muscles in the fields of sensors, controllers, tissue engineering, medical care, and soft robots. Based on the luminous artificial spider silk obtained above, the present invention further prepared a luminous fiber artificial muscle through the following Example 6.

[0114] Embodiment 6:

[0115] The preparation method of fluorescent fiber artificial muscle comprises the following steps:

[0116] Step 1: dissolving 2-acrylamide-2-methylpropanesulfonic acid and N-trimethylolmethyl acrylamide in 1 ml of deionized water, wherein the molar ratio of N-trimethylolmethyl acrylamide to 2-acrylamide-2-methylpropanesulfonic acid is 0.25-0.5, and the total monomer concentration is 3.0-3.8 mol / l, adding 0 and 0.01% MBAA respectively, and then adding 0.068 mg of ammonium persulfate, stirring evenly to obtain a prepolymer solution;

[0117] Step 2: After nitrogen is bubbled into the prepolymer solution of step 1 for 3-5 minutes, the prepolymer solution is injected into a glass capillary with an inner diameter of 0.1-1.0 mm, and 254 nm ultraviolet light with a power of 8 W is used for 4 hours to obtain a spinning solution;

[0118] Step 3: breaking the glass capillary in step 2, and directly stretching and spinning to obtain hydrogel fibers;

[0119] Step 4: Fix the two ends of the fiber obtained in step 3 on a rack, dry and shape it, and finally obtain luminous fiber artificial muscle.

[0120] Fig. 9 This is a picture of the fluorescent fiber artificial muscle contracting under water mist stimulation.

[0121] The fluorescent fiber artificial muscle finally obtained in this embodiment has been tested as follows:

[0122] For the driving and work performance test, a fluorescent fiber artificial muscle with a diameter of 120 microns and containing different hydroxyl monomers was fixed at one end and a 120 mg weight was hung at the other end. It was driven to contract under the stimulation of water mist. Fig.10As shown in the figure, it is explained that as the number of hydroxyl groups increases, the work done by the artificial muscle is greater and the driving stroke is greater.

[0123] For the driving and work performance test, a fluorescent fiber artificial muscle with a diameter of 120 μm, a molar ratio of N-trimethylolmethyl acrylamide to 2-acrylamide-2-methylpropanesulfonic acid of 0.5, a solid content of 3.8 mol / l, and 0.01% MBAA was fixed at one end and different weights were hung at the other end. It was driven to contract under the stimulation of water mist, such as Fig.11 As shown in the figure, it is explained that when the load stress is 256KPa, the artificial muscle does the maximum work.

[0124] For the work performance test, a fluorescent fiber artificial muscle with a diameter of 120 microns and containing different monomer molar ratios and different solid contents was fixed at one end and a weight was hung at the other end. It was driven to contract under the stimulation of water mist. Fig.12 As shown, this figure illustrates that as the proportion of polyhydroxy monomers increases, the solid content increases and MBAA is added, the maximum work done by different fluorescent artificial muscles increases.

[0125] The fluorescent artificial muscle prepared by the present invention can be used for lifting and moving objects in weak light and dark scenes, making up for the shortcomings of traditional artificial muscles in this aspect.

[0126] A variety of materials have been invented and adopted as surgical sutures, including plastics (degradable polyethylene glycol and polylactic acid; non-degradable: nylon and polypropylene), bio-derived proteins (collagen and silk) and metals (stainless steel and nitinol). In order to better promote wound healing, help locate sutures during surgery, facilitate fluorescent image-guided surgery and postoperative bioimaging / diagnosis, and help complex surgeries proceed smoothly, it is necessary to construct luminescent surgical sutures. At present, the methods for constructing luminescent surgical sutures are mainly physical doping of fluorescent dyes, or chemical modification of fluorescent dyes on the surface of surgical threads. These methods are prone to leakage of fluorescent dyes that damage tissues, and fluorescence is also easily quenched. Therefore, it is urgent to prepare surgical sutures with sustainable luminescence and excellent water-resistant mechanical properties. Based on the luminescent artificial spider silk obtained above, the present invention further prepares a luminescent surgical suture through the following examples.

[0127] Embodiment 7:

[0128] The method for preparing a luminous surgical suture comprises the following steps:

[0129] Step 1: dissolving 2-acrylamide-2-methylpropanesulfonic acid and N-trimethylolmethyl acrylamide in 1 ml of deionized water, wherein the molar ratio of N-trimethylolmethyl acrylamide to 2-acrylamide-2-methylpropanesulfonic acid is 0-3, and the total monomer concentration is 1.0-3.8 mol / l, adding 0.01% MBAA, and then adding 0.1 mol% ammonium persulfate, stirring evenly to obtain a prepolymer solution;

[0130] Step 2: After nitrogen is bubbled into the prepolymer solution of step 1 for 3-5 minutes, the prepolymer solution is injected into a glass capillary with an inner diameter of 0.1-1.0 mm, and 254 nm ultraviolet light with a power of 8 W is used for 4 hours to obtain a spinning solution;

[0131] Step 3: breaking the glass capillary in step 2, and directly stretching and spinning to obtain hydrogel fibers;

[0132] Step 4: Fix the two ends of the fiber obtained in step 3 on a rack, dry and shape it, and finally obtain the luminescent hydrogel fiber as the inner core.

[0133] Step 5: The luminescent fiber obtained in step 4 is immersed in the coating solution, taken out and air-dried to obtain a luminescent surgical suture, which includes an inner core and a coating, and the coating is arranged on the surface of the inner core.

[0134] Fig.13 Schematic diagram of the preparation of luminous surgical sutures.

[0135] Embodiment 8:

[0136] The method for preparing a luminous surgical suture comprises the following steps:

[0137] Step 1: dissolving 2-acrylamide-2-methylpropanesulfonic acid and N-trimethylolmethylacrylamide in 1 ml of deionized water, wherein the molar ratio of N-trimethylolmethylacrylamide to 2-acrylamide-2-methylpropanesulfonic acid is 0.5, and the total monomer concentration is 3.8 mol / l, adding 0.01% MBAA, and then adding 0.1 mol% ammonium persulfate, stirring evenly to obtain a prepolymer solution;

[0138] Step 2: After nitrogen is bubbled into the prepolymer solution of step 1 for 3-5 minutes, the prepolymer solution is injected into a glass capillary with an inner diameter of 0.1-1.0 mm, and 254 nm ultraviolet light with a power of 8 W is used for 4 hours to obtain a spinning solution;

[0139] Step 3: breaking the glass capillary in step 2, and directly stretching and spinning to obtain hydrogel fibers;

[0140] Step 4: Fix the two ends of the fiber obtained in step 3 on a rack, dry and shape it, and finally obtain the luminescent hydrogel fiber as the inner core.

[0141] Step 5: The preparation of the coating solution includes: preparing a 5% triacetate cellulose trifluoroacetic acid / dichloromethane (volume ratio = 3:2) solution, preparing a 2% sodium alginate aqueous solution, preparing a 5% polylactic acid dichloromethane solution, preparing a 5% polymethyl acrylate ethyl acetate solution, preparing a 2% chitosan acetic acid / water (volume ratio = 1:50) solution, preparing a 0.5 mol / l calcium chloride aqueous solution, preparing a 10% polyvinyl alcohol 1799 dimethyl sulfoxide solution, preparing a 20% gelatin and 4% chitosan 1% acetic acid solution, preparing a 15% phytate aqueous solution with a pH of 7.4.

[0142] Step 6: The luminescent hydrogel fiber coating includes: immersing the luminescent hydrogel fiber in coating solutions of cellulose triacetate, sodium alginate, polylactic acid and polymethyl acrylate for 3-6 seconds respectively, taking out and air-drying for 12 hours; first immersing the luminescent fiber in a sodium alginate solution for 3-6 seconds, taking out and immediately immersing it in a chitosan solution for 3-6 seconds, taking out and drying it under ambient conditions for 12 hours; first immersing the luminescent fiber in a sodium alginate solution for 3-6 seconds, taking out and immediately immersing it in a calcium chloride solution for 3-6 seconds, taking out and drying it under ambient conditions for 12 hours; first immersing the luminescent fiber in a polyvinyl alcohol 1799 solution for 3-6 seconds, taking out and immediately immersing it in anhydrous ethanol for 1-3 minutes, taking out and drying it under ambient conditions for 12 hours; first immersing the luminescent fiber in a chitosan / gelatin mixed solution for 3-6 seconds, taking out and immediately immersing it in a phytate solution for 5-10 seconds, taking out and drying it under ambient conditions for 12 hours.

[0143] The luminous surgical suture finally obtained in this embodiment has been tested as follows:

[0144] For the swelling performance test, the luminescent hydrogel fibers and the coated surgical sutures were placed in deionized water and swelled to equilibrium. Fig.14 As shown in the figure, it is explained that compared with the uncoated fiber, the anti-swelling performance of the coated surgical thread is improved, among which the anti-swelling performance of the fiber coated with polylactic acid and polymethyl acrylate is the best.

[0145] Mechanical property test: Uncoated fibers and coated surgical sutures with a diameter of 240 μm were subjected to tensile tests before and after swelling (tensile rate was 20 mm / min). Fig.15 As shown in the figure, the mechanical properties of the coated surgical thread are increased compared with the fiber without coating. Among them, the water resistance of the fiber coated with polylactic acid is the best.

[0146] Fluorescence performance test: the uncoated fiber and the coated surgical thread were observed under a fluorescence microscope to observe their fluorescence emission. Fig.16As shown, this figure illustrates that the fluorescence of the coated surgical wire is almost not attenuated compared to the uncoated fiber.

[0147] For cytotoxic activity test, uncoated fibers and polylactic acid-coated fibers were incubated with NIH 3T3 cells for 0, 24, 48, and 72 h, respectively, and cell viability was evaluated using the MTT assay. Fig.17 As shown in the figure, both the uncoated fibers and the polylactic acid coated fibers have good biocompatibility.

[0148] It can be seen from the above Examples 7 and 8 that the present invention first prepares luminescent hydrogel fibers by direct stretching and spinning, and then immerses the fibers in a coating solution for a certain period of time by a dipping method. After the luminescent fibers are taken out, the solvent evaporates quickly, allowing the coating to easily form a film on the surface of the suture. The fibers and the film are combined with each other to protect the internal sutures from external influences, and also improve the smoothness of the suture surface, so that the mechanical properties of the luminescent surgical suture with an inner core and a coating structure are greatly improved, and the luminescent performance is not affected, thereby improving the safety and stability of the surgical sutures during actual use.

[0149] The present invention improves the mechanical properties of the fiber while also improving the water resistance of the fiber by means of coating, providing a new strategy for preparing water-resistant fiber materials. In addition, the preparation method is simple and convenient, and the obtained luminous surgical suture has good mechanical properties, water resistance, and good biocompatibility, meeting clinical needs.

[0150] Protection nets are a very common safety facility in daily life, and have made great contributions to our life, work, production, safety, etc. For example, guardrail nets installed on roads, railways and airports, as well as slope protection nets to prevent rockfall, etc. The use of protection nets can not only reduce the probability of accidents and increase driving safety, but also reduce personal safety hazards and property losses when accidents occur, providing more protection for the safety of life and property.

[0151] The protective net is usually made of strong materials to provide sufficient strength and stability, such as steel, plastic or synthetic fiber. Although these materials can effectively isolate and protect, and have a certain impact resistance, due to the lack of sufficient damping capacity, it is often easy to cause secondary damage to objects that hit the protective net. In addition, the current protective net is invisible at night, and the protective effect will be limited. Therefore, the field of protective net technology urgently needs to develop a new type of protective net to make up for the existing technical gap. Therefore, inspired by spider silk, the present invention prepares a new type of protective net based on hydrogel fiber, and shows excellent mechanical properties, strong fluorescence, high damping and good recovery performance under large deformation. The protective net will show good application potential in the future field of safety protection, such as life preservers for cars driving in the dark and spacecraft landing on the moon or Mars. A fluorescent protective net was further prepared by the following Examples 9 and 10.

[0152] Embodiment 9:

[0153] The preparation method of the fluorescent protection net comprises the following steps:

[0154] Step 1: dissolving 2-acrylamide-2-methylpropane sulfonic acid and polyhydroxy monomer in 1 ml of deionized water, wherein the molar ratio of polyhydroxy monomer to 2-acrylamide-2-methylpropane sulfonic acid is 0-3, and the total monomer concentration is 1.0-3.8 mol / l, adding 0.068 mg of ammonium persulfate, and stirring to obtain a prepolymer solution;

[0155] Step 2: After nitrogen is bubbled into the prepolymer solution of step 1 for 3-5 minutes, the prepolymer solution is injected into a glass capillary with an inner diameter of 0.1-1.0 mm, and 254 nm ultraviolet light with a power of 8 W is used for 4 hours to obtain a spinning solution;

[0156] Step 3: breaking the glass capillary in step 2, and directly stretching and spinning to obtain hydrogel fibers;

[0157] Step 4: Fix the two ends of the fiber obtained in step 3 on a rack, dry and shape it, and finally obtain the fluorescent hydrogel fiber.

[0158] Step 5: Combine and twist the six hydrogel fibers obtained in step 4 into a fluorescent yarn;

[0159] Step 6: Use the fluorescent yarn obtained in step 5 as raw material to weave a fluorescent protective net with a warp density of 1 yarn per inch and a weft density of 2 yarns per inch. The warp length is 15 cm and the weft length is 20 cm.

[0160] The hydrogel fibers obtained in this example were subjected to the following tests:

[0161] Damping capacity calculation, the hydrogel fibers with a diameter of 15 μm and containing different hydroxyl monomers were subjected to a "loading-unloading" test under the condition of 25% air humidity, such as Fig.18 As shown in (b), the damping capacity is calculated from the ratio of the damping energy (the area contained by the loading and unloading curves) to the loading energy (the area contained by the loading curve and the dotted line). Fig.18 As shown in (a), the damping capacity of the fluorescent hydrogel fiber is 90%.

[0162] Cyclic "loading-unloading" damping capacity and stress test, the diameter of 15 microns was subjected to 5 cycles of "loading-unloading" test, after each test, the fiber was shrunk to its original length under high humidity, and the stress and damping capacity were calculated, and then the next test was carried out under the condition of 25% relative humidity. Fig.19 As shown in the figure, the damping capacity and stress of the fluorescent hydrogel fiber are almost not lost after multiple cycles.

[0163] Cyclic super shrinkage test, the fluorescent hydrogel fiber with a diameter of 100 microns was subjected to 5 cycles of "loading-unloading" test, after each experiment, the fiber was shrunk under high humidity, and the shrinkage rate was calculated, and then the next experiment was carried out under the condition of relative humidity of 25%. Fig. 20 As shown in the figure, the super shrinkage performance of the fluorescent hydrogel fiber is almost not lost after multiple cycles.

[0164] Embodiment 10:

[0165] The preparation method of the fluorescent protection net comprises the following steps:

[0166] Step 1: 2-acrylamide-2-methylpropanesulfonic acid and N-trimethylolmethylacrylamide are dissolved in 1 ml of deionized water, wherein the molar ratio of N-trimethylolmethylacrylamide to 2-acrylamide-2-methylpropanesulfonic acid is 0.5, and the total monomer concentration is 3.8 mol / l, 0.01% of MBAA and 0.068 mg of ammonium persulfate are added respectively, and the mixture is stirred to obtain a prepolymer solution;

[0167] Step 2: After nitrogen is bubbled into the prepolymer solution of step 1 for 3-5 minutes, the prepolymer solution is injected into a glass capillary with an inner diameter of 0.1-1.0 mm, and 254 nm ultraviolet light with a power of 8 W is used for 4 hours to obtain a spinning solution;

[0168] Step 3: breaking the glass capillary in step 2, and directly stretching and spinning to obtain hydrogel fibers;

[0169] Step 4: Fix the two ends of the fiber obtained in step 3 on a rack, dry and shape it, and finally obtain the luminescent hydrogel fiber;

[0170] Step 5: Combine and twist the six hydrogel fibers obtained in step 4 into a fluorescent yarn;

[0171] Step 6: Use the fluorescent yarn obtained in step 5 as raw material to weave a fluorescent protective net with a warp density of 1 yarn per inch and a weft density of 2 yarns per inch. The warp length is 15 cm and the weft length is 20 cm.

[0172] The fluorescent protection net finally obtained in this embodiment has been tested as follows:

[0173] High-speed object interception test: a 240g toy airplane flies towards a fluorescent protection net at a speed of 90cm / s in dark conditions. Fig.21 As shown, the toy airplane is successfully intercepted by the protective net, the fluorescent protective net is greatly deformed, and then recovers its original shape after being exposed to 60% relative humidity. This figure illustrates that the fluorescent protective net has good cushioning and recovery properties.

[0174] The present invention successfully prepared fluorescent hydrogel fiber yarn with long-lasting and stable luminescence and strong mechanical properties. The yarn density and fabric density can be adjusted as needed to prepare a fluorescent protective net, achieving customizability.

[0175] The fluorescent protective net prepared by the present invention can be used as a lifesaver for objects moving at high speed in weak light and dark scenes, and is expected to be applied to protective nets for roads, railways and airports, isolation nets to prevent falling rocks and falling objects, and aerospace and other fields.

[0176] Based on the above technical concepts and embodiments, the present invention provides a method for preparing luminescent artificial spider silk fibers. The method achieves the regulation of the spinnability, mechanical properties and fluorescence properties of the luminescent artificial spider silk by changing the concentration and ratio of organic acid derivatives and polyhydroxy monomers, and successfully prepares artificial spider silk with high strength, good spinnability and long-lasting and stable luminescence. At the same time, the philtrum muscle can be used in multiple scenarios by utilizing its own luminescence characteristics. Furthermore, direct stretch spinning is combined with coating technology to prepare a surgical suture with high mechanical properties, strong water resistance and luminescence, which can be well used in the positioning of surgical sutures during and after complex surgeries and the visualization management of wounds, with attached Fig. 22The images of intact and broken fluorescent surgical sutures under the skin of mice at 365nm and in daylight are shown, the arrow indicates the position of the fluorescent surgical suture, and the dotted circle indicates the position where the fluorescent surgical suture is broken. And the method for preparing the luminous surgical suture provided by the present invention is simple, convenient, low-cost and environmentally friendly. Furthermore, the present invention first synthesizes several strands of the obtained fluorescent hydrogel fibers into a strand and twists them to form a fluorescent yarn, and then weaves the warp and weft yarns into a fluorescent protective net. The present invention can flexibly adjust the weaving density according to different application scenarios, and the protective net can be conveniently arranged in high-rise buildings, roads, bridges and decks. Since the fluorescent hydrogel fiber also has the properties of high damping and shape memory under high humidity, the protective net prepared by the present invention can play a good buffering role for high-speed moving objects and can be reused. Its own luminous properties enable it to be used in weak light or at night, overcoming the disadvantage that the general protective net is only used under strong light.

[0177] It should be further explained that the above embodiments are only used to understand the technical concept and technical solution of the present invention, and are not used to limit the protection scope of the present invention. Any obvious adjustments or modifications made to the above technical solutions that belong to the technical concept of the present invention should fall within the protection scope of the present invention.

Claims

1. A method for preparing luminous artificial spider silk, characterized in that The following steps are involved: Step 1: dissolving an organic acid derivative and a polyhydroxy monomer in deionized water, adding a crosslinking agent and an initiator, and stirring to obtain a prepolymer solution; Step 2: Blowing an inert gas into the prepolymer solution in step 1 to obtain a spinning solution through free radical polymerization; Step 3: directly spinning the spinning solution in step 2 to obtain luminous artificial spider silk or hydrogel fiber.

2. The preparation method according to claim 1, characterized in that: The organic acid derivative can be replaced by one of 2-acrylamide-2-methylpropanesulfonic acid, acrylic acid, acrylamide, methacrylic acid, propylenesulfonic acid, cis-acrylphosphoric acid, N-acryloylglycine, N-acryloylalanine, N-acryloylbutyric acid, and N-(2-amino-2-oxoethyl)acrylamide; The polyhydroxy monomer is one of the following: N-hydroxyethyl acrylamide, N-dihydroxymethyl methacrylamide, N-trihydroxymethyl methacrylamide, polyvinyl alcohol; The initiator is one of ammonium persulfate, potassium persulfate, 2-hydroxy-2-methyl-1-phenylacetone, and α-ketoglutaric acid, accounting for 0.1-0.5 mol% of the total monomers; The cross-linking agent is N,N'-methylenebisacrylamide (MBAA), accounting for 0-0.05 mol% of the total monomers.

3. The preparation method according to claim 1, characterized in that: The inert gas blown in can be one of nitrogen and argon, and the blowing time is 1-10 minutes.

4. The preparation method according to claim 1, characterized in that: The prepolymer solution is injected into a tubular mold such as a glass capillary for polymerization.

5. The preparation method according to claim 1, characterized in that: The initiation conditions of free radical polymerization can be one of heating polymerization and ultraviolet polymerization; The prepolymer solution is polymerized under ultraviolet light with a power of 8-20 W for 0.5-6 hours. The prepolymer solution is heated at a temperature of 40-60° C. for 1-12 hours.

6. The preparation method according to claim 1, characterized in that: The spinning method may be one of the following: breaking off a tubular die such as a glass capillary and directly stretching and spinning, using an iron rod dipped in spinning solution to directly stretch and spin, or dry spinning; Direct spinning can produce luminous artificial spider silk with a diameter of 5-300 microns.

7. The preparation method according to claim 1, characterized in that: The method comprises the steps of shaping and drying, wherein the shaping time of the luminous artificial spider silk or hydrogel fiber is 30-300 seconds; The drying condition of the luminous artificial spider silk or hydrogel fiber is 30-100° C. for 1-15 hours.

8. A method for preparing a luminous surgical suture, characterized in that: The luminous surgical suture comprises an inner core and a coating, and comprises the following steps: Invading the hydrogel fiber obtained by any one of claims 1 to 7 as an inner core into the coating solution, taking it out and drying it to obtain a luminous surgical suture; The coating solution includes cellulose triacetate (CTA), sodium alginate (SA), polylactic acid (PLA), sodium alginate / chitosan (SA / CS), sodium alginate / Ca 2+ (SA / Ca 2+ ), any one of the solutions of polymethyl acrylate (PMA), polyvinyl alcohol 1799 (PVA1799), gelatin / chitosan / phytate (GEL / CS / SP); the time for the inner core hydrogel fiber to invade the coating solution is 3-10 seconds; the inner core hydrogel fiber is taken out from the coating solution and dried for 1-12 hours.

9. The method for preparing the luminous surgical suture according to claim 8, characterized in that: The diameter of the inner core hydrogel fiber is 50-220 μm, and the thickness of the coating is 10-30 μm.

10. A method for preparing a fluorescent protection net, characterized in that The following steps are involved: Step 1: combining and twisting the hydrogel fibers obtained by any one of claims 1 to 7 into fluorescent yarns; Step 2: Weaving the fluorescent yarn obtained in step 1 into a fluorescent protective net according to a certain fabric density; The fluorescent protection net woven according to a certain fabric density refers to: the warp density is 1 yarn per inch, the weft density is 2 yarns per inch, the warp length is 15 cm, and the weft length is 20 cm.