Photoelectric composite cable for coal mine and manufacturing method thereof
By using composite multivariate flame retardant additives and surface modification mullite fiber reinforcement in polypropylene, the flame retardant and mechanical properties of photoelectric composite cables are improved, and the problem of insufficient flame retardant performance of polypropylene in coal mine environments is solved. , realizes the safety and use requirements of cables.
Patent Information
- Application Number
- CN202411119376.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
When polypropylene is used in photoelectric composite cables in complex environments such as coal mines, it has poor flame retardant performance and insufficient mechanical strength. The existing inorganic flame retardant is not modified. Conventional phosphorus-based small-molecule flame retardant is prone to volatilization and migration, resulting in Inadequate long-term effectiveness.
Using composite multivariate flame retardant additives and surface-modified mullite fiber reinforcement, the expanded flame retardant and macromolecular polyethersulfone modified fibers are added to polypropylene to form high efficiency The flame retardant and reinforced materials improve the flame retardant and mechanical properties of the cable.
It has achieved significant improvements in the long-term flame retardant performance and mechanical mechanical properties of the cable, avoided the precipitation of flame retardant and decreased mechanical properties, and met the safety and use needs of photoelectric composite cables for coal mines.
Smart Images

Figure CN119008103A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cables, and in particular to a photoelectric composite cable for coal mines and a manufacturing method thereof. Background Art
[0002] With the rapid development of science and technology, optoelectronic composite cables, as a new type of cable that integrates power transmission and optical signal transmission, are gradually becoming an important infrastructure in the field of modern communications and energy transmission. Optoelectronic composite cables not only improve transmission efficiency, but also reduce wiring costs and maintenance difficulties, providing strong support for the construction of intelligent cities and the rapid development of the information society. In the composition of optoelectronic composite cables, the sheath layer is the protective barrier of the cable, and the selection of its material is crucial.
[0003] Polypropylene has good electrical insulation properties, which is an important basis for its use as a cable sheath material. In optoelectronic composite cables, the power transmission part requires strict electrical insulation to prevent current leakage and short circuits, while the high insulation strength and anti-puncture capability of polypropylene can effectively prevent current leakage and ensure the electrical safety of the cable. At the same time, the lower dielectric loss and dielectric constant of polypropylene means less energy loss and low signal attenuation during transmission, which is conducive to maintaining the stable transmission of electrical and optical signals.
[0004] However, with the increasing application of cables, special industries such as coal mines have higher and higher safety requirements for cables. However, due to its linear structure, polypropylene has poor flame retardancy and a limiting oxygen index of about 18%, making it an extremely flammable material. In addition, the mechanical strength of polypropylene is not satisfactory, which makes it unable to meet the mechanical support required when cables are installed and used in complex environments such as mines and are subjected to external forces. Therefore, it is urgent to improve the comprehensive properties of polypropylene, such as flame retardancy.
[0005] In the prior art, polypropylene is often flame-retarded by adding inorganic flame retardants such as magnesium hydroxide. However, the flame-retardant modification effect of inorganic flame retardants is not good, and a large amount of addition is required to show a certain effect, which will have a negative impact on the mechanical strength of polypropylene. Therefore, simple inorganic flame retardant filling actually has a large defect in the flame-retardant modification of polypropylene, and conventional phosphorus-based halogen-free small molecule flame retardants are easy to volatilize and migrate during use, resulting in the long-term effectiveness not being guaranteed, and there are still deficiencies in practical application. Summary of the invention
[0006] 1. Technical issues to be solved
[0007] In view of the deficiencies in the prior art, the present invention provides a photoelectric composite cable for coal mines and a method for manufacturing the same.
[0008] (II) Technical solution
[0009] A photoelectric composite cable for coal mines, comprising a cable core, a wrapping layer, and a sheath layer from the inside to the outside; the sheath layer is made by extruding a sheath composite material on the outside of the wrapping layer, and the sheath composite material is made of raw materials including the following parts by weight:
[0010] Polypropylene 85-95 parts, compatibilizer 10-15 parts, composite multi-component flame retardant additive 3-6 parts, mullite fiber reinforcement 2-4 parts, lubricant 0.5-1.5 parts, antioxidant 0.5-1 parts;
[0011] The preparation method of the sheath composite material is as follows:
[0012] After weighing each raw material according to the weight proportion, put it into a mixer, stir and mix it at a speed of 1000-1500r / min for 20-30min, and then feed the mixed material into a twin-screw extruder through a feeding hopper, control the extruder temperature to 180-220℃, the screw speed to 50-60rpm, and extrude and granulate.
[0013] More preferably, the compatibilizer is maleic anhydride grafted polypropylene or maleic anhydride grafted polyethylene.
[0014] Further preferably, the preparation method of the composite multi-element flame retardant additive comprises the following steps:
[0015] Step 1, add pyrimidine-4,6-dicarboxylic acid and 1,4-dioxane to a reactor filled with nitrogen, start stirring, and after complete dissolution, continue to add triglycidyl isocyanurate and a catalyst to the reactor. After the addition is complete, gradually increase the temperature to 70-80°C, stir continuously for 7-9 hours, cool down and discharge the material to form a flame retardant intermediate material;
[0016] Step 2: Add the flame retardant intermediate material, ethylene chlorophosphate and tetrahydrofuran into the reactor, stir and mix, introduce nitrogen to expel the air, then gradually increase the temperature to 60-65°C, keep warm for 1-2 hours, add the acidifying agent, continue stirring for 2-4 hours, cool and discharge the material, and you can get a composite multi-element flame retardant additive.
[0017] Further preferably, in step 1, the catalyst is at least one of tetrabutylammonium hydrogen sulfate, tetrabutylammonium bromide, tetramethylammonium bromide or N,N-dimethylbenzylamine.
[0018] Further preferably, in the step 1, the molar ratio of pyrimidine-4,6-dicarboxylic acid to triglycidyl isocyanurate is 1-1.5:1.
[0019] Further preferably, in the step 2, the acidifying agent is triethylamine.
[0020] In the above technical scheme, a phase transfer catalyst is first used to catalyze the esterification ring-opening of the substituted carboxyl group in the pyrimidine-4,6-dicarboxylic acid structure and the carboxyl group in the triglycidyl isocyanurate structure, and continuously polymerize to form a macromolecular flame retardant intermediate material connected by ester bonds. Since substituted hydroxyl groups are generated during the esterification ring-opening process, they can undergo further condensation reaction with the phosphorus oxychloride group in the cyclic chloroethylene phosphate structure under the action of an acidifying agent, thereby obtaining a multi-element flame retardant material containing nitrogen and phosphorus in the structure, that is, a composite multi-element flame retardant additive. The pyrimidine ring contained in its structure can be used as a carbon source, and combined with a nitrogen source and a phosphorus source, it can form an intumescent flame retardant.
[0021] Further preferably, the preparation method of the mullite fiber reinforcement comprises the following steps:
[0022] Step ①, adding mullite fiber to toluene, ultrasonicating for 20-30 minutes to form a dispersion, then adding 2-chloroethyl isocyanate and dibutyltin dilaurate to the dispersion, after the addition, gradually raising the temperature to 60-70°C, and then maintaining the temperature for 4-8 hours, centrifuging and separating the solid material to obtain a modified fiber material;
[0023] Step ②, disperse the modified fiber material in N, N-dimethylformamide, then add the terminal hydroxyl polyether sulfone and sodium hydroxide solution under stirring conditions, after adding, control the temperature to 70-80°C, continue stirring for 6-9 hours, and centrifuge to separate the product to obtain the mullite fiber reinforcement.
[0024] Further preferably, in step ②, the mass ratio of the modified fiber material to the hydroxy-terminated polyethersulfone is 1:5-15.
[0025] Further preferably, in step ②, the mass fraction of the sodium hydroxide solution is 10-20%.
[0026] In the above technical scheme, the hydroxyl groups on the surface of the mullite fiber undergo an amine esterification reaction with the isocyanate groups in the 2-chloroethyl isocyanate structure under the catalysis of dibutyltin dilaurate, thereby modifying the surface of the mullite fiber with halogen substituents, i.e., modified fiber material. Subsequently, under the action of sodium hydroxide, the hydroxyl groups in the terminal hydroxyl polyether sulfone structure are substituted, thereby modifying the surface of the mullite fiber with macromolecular polyether sulfone to obtain a mullite fiber reinforcement material.
[0027] A method for manufacturing a photoelectric composite cable for coal mines, comprising the following steps:
[0028] Twisting three insulated wire cores and an optical unit to form a cable core, then placing it in a cabling machine, filling the gaps with non-woven fabric, then wrapping the cable core with a polyester tape to form a wrapping layer, and then extruding the sheath composite material and coating it on the outside of the insulation layer to form a sheath layer.
[0029] (III) Beneficial technical effects
[0030] (1) The present invention first prepares a composite multi-component flame retardant additive containing multi-component flame retardant elements in its structure as an additive to modify polypropylene. Since the composite multi-component flame retardant additive is an expandable flame retardant that integrates a carbon source, an acid source and a gas source, it can quickly form an expandable carbon layer to wrap the cable when it burns, thereby preventing the burning from continuing. Since the composite multi-component flame retardant additive itself is a macromolecular structure and can interact with a compatibilizer during a high-temperature melting process, thereby forming an intertwined molecular structure with polypropylene, the precipitation problem of the flame retardant can be effectively avoided, thereby ensuring the long-term flame retardant performance of the cable.
[0031] (2) The present invention prepares mullite fiber with surface modification of macromolecular polyethersulfone as a modifier to enhance and modify polypropylene. First, the substituted hydroxyl group at the other end of the polyethersulfone molecular chain can interact with the maleic anhydride of the compatibilizer, thereby forming a micro-connection network at the interface of the mullite fiber and the polypropylene matrix. This can not only improve the compatibility of the mullite fiber and the polypropylene, and efficiently utilize the advantages of the mullite fiber to enhance the mechanical properties of the polypropylene, but also utilize the rigid structure in the polyethersulfone structure to improve the rigidity and density of the polypropylene molecular chain, thereby further enhancing the mechanical properties of the polypropylene and meeting the use requirements of the optoelectronic composite cable. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0033] Figure 1 This is the infrared analysis test chart of the composite multi-component flame retardant additive. DETAILED DESCRIPTION
[0034] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0035] Preparation Example 1
[0036] Preparation of composite multi-component flame retardant additives:
[0037] Step 1: Add 0.3 g of pyrimidine-4,6-dicarboxylic acid and 1,4-dioxane to a reactor filled with nitrogen, start stirring, and after complete dissolution, continue to add 0.5 g of triglycidyl isocyanurate and 0.1 g of tetrabutylammonium bromide to the reactor. After the addition is complete, gradually increase the temperature to 75°C, stir continuously for 8 hours, cool and discharge the material to form a flame retardant intermediate material;
[0038] Step 2: Add 0.6 g of flame retardant intermediate material, 0.2 g of ethylene chlorophosphate and tetrahydrofuran into the reactor, stir to mix, introduce nitrogen to expel the air, then gradually increase the temperature to 65°C, keep warm for 1 hour, add 0.5 g of triethylamine, continue stirring for 3 hours, cool and discharge the material to obtain a composite multi-component flame retardant additive.
[0039] Figure 1 This is the infrared analysis test chart of the composite multi-element flame retardant additive, where 3302cm -1 The absorption peak at 2800-3000cm is the characteristic absorption peak of hydroxyl group. -1 The absorption peak at 1749 cm is the characteristic absorption peak of CH in methylene. -1 The absorption peak at 1697 cm is the characteristic absorption peak of C=O of the ester group. -1 The absorption peak at 1298 cm is the characteristic absorption peak of C=O in the heterocyclic ring of isocyanuric acid. -1 The absorption peak that appears at is the characteristic absorption peak of P=O.
[0040] Preparation Example 2
[0041] Preparation of mullite fiber reinforcement:
[0042] Step ①, adding 1.5g of mullite fiber to toluene, ultrasonicating for 30min to form a dispersion, then adding 2.4g of 2-chloroethyl isocyanate and 0.02g of dibutyltin dilaurate to the dispersion, after the addition, gradually raising the temperature to 65°C, and then maintaining the temperature for 6h, centrifuging and separating the solid material to obtain a modified fiber material;
[0043] Step ②, disperse 1.2g of modified fiber material in N,N-dimethylformamide, then add 16g of terminal hydroxyl polyether sulfone and 20mL of 15% sodium hydroxide solution under stirring. After adding, control the temperature to 75°C, continue stirring for 8h, and centrifuge to separate the product to obtain mullite fiber reinforcement.
[0044] Example 1
[0045] Preparation of sheath composite material:
[0046] According to the weight proportions, 85 parts of polypropylene, 10 parts of maleic anhydride grafted polypropylene, 3 parts of composite multi-component flame retardant additives, 2 parts of mullite fiber reinforcement, 0.5 parts of lubricant polyethylene wax and 0.5 parts of antioxidant 1010 are put into a mixer, stirred and mixed at a speed of 1000r / min for 20 minutes, and then the mixture is fed into a twin-screw extruder through a feeding hopper, the extruder temperature is controlled at 200°C, the screw speed is controlled at 50rpm, and extrusion granulation is performed.
[0047] The preparation method of the composite multi-element flame retardant additive is shown in Preparation Example 1; the preparation method of the mullite fiber reinforcement is shown in Preparation Example 2, and the same is true for the following.
[0048] Example 2
[0049] Preparation of sheath composite material:
[0050] According to the weight proportions, 90 parts of polypropylene, 12 parts of maleic anhydride grafted polypropylene, 5 parts of composite multi-component flame retardant additives, 3.5 parts of mullite fiber reinforcement, 1.2 parts of lubricant polyethylene wax and 0.6 parts of antioxidant 1010 were put into a mixer, stirred and mixed at a speed of 1200r / min for 30 minutes, and then the mixture was fed into a twin-screw extruder through a feeding hopper, the extruder temperature was controlled at 200°C, the screw speed was controlled at 50rpm, and extrusion granulation was performed.
[0051] Example 3
[0052] Preparation of sheath composite material:
[0053] According to the weight proportions, 95 parts of polypropylene, 15 parts of maleic anhydride grafted polypropylene, 6 parts of composite multi-element flame retardant additives, 4 parts of mullite fiber reinforcement, 1.5 parts of lubricant polyethylene wax and 1 part of antioxidant 1010 were put into a mixer, stirred and mixed at a speed of 1500r / min for 30 minutes, and then the mixture was fed into a twin-screw extruder through a feeding hopper, the extruder temperature was controlled at 220°C, the screw speed was controlled at 50rpm, and extrusion granulation was performed.
[0054] Comparative Example 1
[0055] Preparation of sheath composite material:
[0056] According to the weight proportions, 90 parts of polypropylene, 12 parts of maleic anhydride grafted polypropylene, 5 parts of composite multi-component flame retardant additives, 3.5 parts of mullite fiber, 1.2 parts of lubricant polyethylene wax and 0.6 parts of antioxidant 1010 were put into a mixer, stirred and mixed at a speed of 1200r / min for 30 minutes, and then the mixture was fed into a twin-screw extruder through a feeding hopper, the extruder temperature was controlled at 200°C, the screw speed was controlled at 50rpm, and extrusion granulation was performed.
[0057] Comparative Example 2
[0058] Preparation of sheath composite material:
[0059] According to the weight proportions, 90 parts of polypropylene, 12 parts of maleic anhydride grafted polypropylene, 5 parts of composite multi-component flame retardant additives, 1.2 parts of lubricant polyethylene wax and 0.6 parts of antioxidant 1010 are put into a mixer, stirred and mixed at a speed of 1200r / min for 30 minutes, and then the mixture is fed into a twin-screw extruder through a feeding hopper, the extruder temperature is controlled at 200°C, the screw speed is controlled at 50rpm, and extrusion granulation is performed.
[0060] Comparative Example 3
[0061] Preparation of sheath composite material:
[0062] According to the weight proportions, 90 parts of polypropylene, 12 parts of maleic anhydride grafted polypropylene, 5 parts of cyclic vinyl chlorophosphate, 3.5 parts of mullite fiber reinforcement, 1.2 parts of lubricant polyethylene wax and 0.6 parts of antioxidant 1010 were put into a mixer, stirred and mixed at a speed of 1200r / min for 30min, and then the mixture was fed into a twin-screw extruder through a feeding hopper, the extruder temperature was controlled at 200°C, the screw speed was controlled at 50rpm, and extrusion granulation was performed.
[0063] Test Case
[0064] The sheath composite materials in Examples 1 to 3 and Comparative Examples 1 to 3 were made into test samples of corresponding test specifications, and various performance tests were performed. The results are recorded in Table 1:
[0065] Table 1 - Test results
[0066] Tensile Strength Impact strength Limiting oxygen index Example 1 34.7MPa <![CDATA[29.4kJ / m 2 ]]> 32.1% Example 2 35.2MPa <![CDATA[29.9kJ / m 2 ]]> 32.2% Example 3 35.0MPa <![CDATA[29.5kJ / m 2 ]]> 32.0% Comparative Example 1 31.5MPa <![CDATA[25.1kJ / m 2 ]]> 30.5% Comparative Example 2 22.4MPa <![CDATA[18.8kJ / m 2 ]]> 28.8% Comparative Example 3 33.8MPa <![CDATA[29.0kJ / m 2 ]]> 23.9%
[0067] Note: The tensile strength test refers to the standard GB / T 10401.1-2006; the impact strength test refers to the standard GB / T14152-2001; the limiting oxygen index test refers to the standard GB / T 2406.2-2009. The test samples are placed at room temperature for 3 months before testing.
[0068] According to the test results, the sheath composite material prepared by adding the composite multi-component flame retardant additive and the mullite fiber reinforcement obviously has excellent mechanical strength and flame retardant properties.
[0069] After replacing the mullite fiber reinforcement with mullite fiber that has not been surface modified, on the one hand, due to the problem of interface compatibility, the mullite fiber cannot effectively exert its advantages. On the other hand, the polyethersulfone molecular chain is lost and the micro-cross-linking structure cannot be formed, resulting in a decrease in the mechanical properties of the material. In addition, since the sulfur element in the polyethersulfone structure also has a flame retardant effect, the flame retardant performance also decreases slightly.
[0070] After the mullite fiber is directly removed, the advantages of the mullite fiber cannot be utilized, resulting in a significant reduction in the mechanical properties of the material. Moreover, it can be concluded from the test data that the addition of mullite fiber has a positive effect on the flame retardant properties of the material.
[0071] After replacing the composite multi-flame retardant additive with a small molecule phosphorus-containing flame retardant ethylene chlorophosphate, on the one hand, volatilization migration occurs during long-term storage, and on the other hand, the phosphorus-based flame retardant is too single and does not have the advantages of an expanding flame retardant. Therefore, the effect of adding a small amount is not significant, resulting in a significant decrease in the flame retardant properties of the material.
[0072] The sheath composite material in Example 2 of the present invention is used to prepare an optoelectronic composite cable for coal mines, and the preparation method is as follows;
[0073] Twisting three insulated wire cores and an optical unit to form a cable core, then placing it in a cabling machine, filling the gaps with non-woven fabric, then wrapping the cable core with a polyester tape to form a wrapping layer, and then extruding the sheath composite material and coating it on the outside of the insulation layer to form a sheath layer.
[0074] Based on the ideal embodiment of the present invention, through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.
Claims
1. A photoelectric composite cable for coal mines, characterized in that: The cable core, the wrapping layer and the sheath layer are sequentially included from the inside to the outside; the sheath layer is obtained by extruding the sheath composite material on the outside of the wrapping layer; the sheath composite material is made of raw materials including the following parts by weight: Polypropylene 85-95 parts, compatibilizer 10-15 parts, composite multi-component flame retardant additive 3-6 parts, mullite fiber reinforcement 2-4 parts, lubricant 0.5-1.5 parts, antioxidant 0.5-1 parts; The preparation method of the sheath composite material is as follows: After weighing each raw material according to the weight proportion, put it into a mixer, stir and mix it at a speed of 1000-1500r / min for 20-30min, and then feed the mixed material into a twin-screw extruder through a feeding hopper, control the extruder temperature to 180-220℃, the screw speed to 50-60rpm, and extrude and granulate.
2. The optoelectronic composite cable for coal mine according to claim 1, characterized in that: The compatibilizer is maleic anhydride grafted polypropylene or maleic anhydride grafted polyethylene.
3. The optoelectronic composite cable for coal mine according to claim 1, characterized in that: The preparation method of the composite multi-element flame retardant additive comprises the following steps: Step 1, add pyrimidine-4,6-dicarboxylic acid and 1,4-dioxane to a reactor filled with nitrogen, start stirring, and after complete dissolution, continue to add triglycidyl isocyanurate and a catalyst to the reactor. After the addition is complete, gradually increase the temperature to 70-80°C, stir continuously for 7-9 hours, cool down and discharge the material to form a flame retardant intermediate material; Step 2: Add the flame retardant intermediate material, ethylene chlorophosphate and tetrahydrofuran into the reactor, stir and mix, introduce nitrogen to expel the air, then gradually increase the temperature to 60-65°C, keep warm for 1-2 hours, add the acidifying agent, continue stirring for 2-4 hours, cool and discharge the material, and you can get a composite multi-element flame retardant additive.
4. The optoelectronic composite cable for coal mine according to claim 3, characterized in that: In the step 1, the catalyst is at least one of tetrabutylammonium hydrogen sulfate, tetrabutylammonium bromide, tetramethylammonium bromide or N,N-dimethylbenzylamine.
5. The optoelectronic composite cable for coal mine according to claim 3, characterized in that: In the step 1, the molar ratio of pyrimidine-4,6-dicarboxylic acid to triglycidyl isocyanurate is 1-1.5:
1.
6. The optoelectronic composite cable for coal mine according to claim 3, characterized in that: In the step 2, the acidifying agent is triethylamine.
7. The optoelectronic composite cable for coal mine according to claim 1, characterized in that: The preparation method of the mullite fiber reinforcing agent comprises the following steps: Step ①, adding mullite fiber to toluene, ultrasonicating for 20-30 minutes to form a dispersion, then adding 2-chloroethyl isocyanate and dibutyltin dilaurate to the dispersion, after the addition, gradually raising the temperature to 60-70°C, and then maintaining the temperature for 4-8 hours, centrifuging and separating the solid material to obtain a modified fiber material; Step ②, disperse the modified fiber material in N, N-dimethylformamide, then add the terminal hydroxyl polyether sulfone and sodium hydroxide solution under stirring conditions, after adding, control the temperature to 70-80°C, continue stirring for 6-9 hours, and centrifuge to separate the product to obtain the mullite fiber reinforcement.
8. The optoelectronic composite cable for coal mine according to claim 7, characterized in that: In the step ②, the mass ratio of the modified fiber material to the hydroxy-terminated polyethersulfone is 1:5-15.
9. The optoelectronic composite cable for coal mine according to claim 7, characterized in that: In the step ②, the mass fraction of the sodium hydroxide solution is 10-20%.
10. A method for manufacturing a photoelectric composite cable for coal mines as claimed in claim 1, characterized in that: The following steps are involved: Twisting three insulated wire cores and an optical unit to form a cable core, then placing it in a cabling machine, filling the gaps with non-woven fabric, then wrapping the cable core with a polyester tape to form a wrapping layer, and then extruding the sheath composite material and coating it on the outside of the insulation layer to form a sheath layer.
Citation Information
Cited By
Wear-resistant high-toughness polypropylene material and preparation method thereof
CN120365657A
Mining flame-retardant cross-linked polyethylene insulated power cable
CN121601332A