Preparation method of multi-fold mechanically-enhanced self-repairing supercapacitor
Through pre-stretching strategy and liquid metal modification, the mechanical and self-healing properties of carbon nanotube-PEDOT:PSS composite membrane are improved, and the problem of poor mechanical properties of traditional micro supercapacitors is solved, achieving high energy density and large-scale Integrated for wearable devices and sensors.
Patent Information
- Application Number
- CN202411276960.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional micro-supercapacitors have poor mechanical properties and cannot meet the functional needs of high energy density, large-scale integration and bendability, especially in wearable microelectronic devices.
Pre-stretching strategy to prepare a composite film of liquid metal-modified carbon nanotubes-poly(3,4 ethylene dioxythiophene) (PEDOT) and polystyrene sulfonic acid (PSS) to improve the mechanical properties of electrode materials through strong interactions and self-healing, and enhance stretchability and specific capacity through wrinkle structure.
A flexible and stretchable electrode material is realized, which improves the mechanical properties and self-healing ability of the electrode material, solves the problems of low energy density and difficulty in integration of traditional micro supercapacitors, and broadens the application scenarios, especially in wearable devices and sensor fields.
Smart Images

Figure HDA0005040495430000011 
Figure HDA0005040495430000012 
Figure HDA0005040495430000013
Abstract
Description
Technical Field
[0001] The present invention specifically relates to a method for preparing a multi-fold mechanically enhanced self-repairing supercapacitor, and belongs to the field of supercapacitors. Background Art
[0002] With the rapid development of society, the fields of healthcare, automobile industry, aerospace, industrial automatic robots, portable and wearable electronic products have risen rapidly. The rise of microelectronic devices urgently requires micro energy devices to match them. Micro supercapacitors (MSCs) have become mobile energy storage devices with great development prospects due to their advantages such as fast charging and discharging speed, high power density and long life, and have attracted widespread attention. However, low energy density and difficulty in integration have seriously restricted the development of MSCs. Scientists have conducted a lot of research on electrode materials, electrolytes and assembly strategies. However, due to the poor conductivity of electrode materials, unsatisfactory specific capacitance and low accessible surface area, this problem has not been well solved. In particular, traditional MSCs have poor mechanical properties, lack of anti-bending and healing capabilities, so current MSCs cannot meet the functional requirements of wearable microelectronic devices in terms of high energy density, large-scale integration, bendability and other aspects. Therefore, designing electrode materials that are easy to integrate on a large scale, have high energy density and have both self-healing properties and mechanical toughness is the key to achieving micro supercapacitors to meet the energy needs of microelectronic devices and achieve high energy output. Summary of the invention
[0003] Carbon nanotubes as electrode materials have good electrical conductivity and fast charge transfer capabilities, but CNTs themselves are difficult to form cross-linked structures, resulting in poor mechanical properties of the electrode film. At the same time, CNTs are double-layer energy storage materials, and the capacitance provided by electron adsorption is limited. Therefore, CNTs are often combined with other materials as electrode materials to improve their mechanical and electrochemical properties. Liquid metal (LM) has high electrical conductivity (σ = 3.4 × 106 S m -1 ), stretchability, self-healing and biocompatibility, etc., which have attracted widespread attention in recent years. Due to the large surface tension of LM itself, LM is difficult to be composited with other materials.
[0004] Here, we propose a pre-stretching strategy to prepare liquid metal-modified carbon nanotube-poly(3,4-ethylenedioxythiophene) (PEDOT) and polystyrene sulfonic acid (PSS) composite films (LM-CNT-PEDOT:PSS) with multi-fold strong mechanical and healing properties. In the presence of PEDOT:PSS, the oxygen-containing functional groups on the surface of CNTs can interact strongly with the native oxide layer on the surface of LM, thereby obtaining a flexible and stretchable electrode. The introduction of LM improves the mechanical properties of the composite film, and the self-healing property makes the electrode material easy to integrate on a large scale. The introduction of PEDOT:PSS can not only promote the formation of CNTs film and the combination of LM and CNTs, but also improve the specific capacity of the electrode material. In addition, the wrinkled structure can increase the active specific surface area per unit area, solving the problem of low area energy density when the smoothly stacked CNTs film is used as a microelectrode. The construction of the wrinkled structure also enhances the stretchability. The introduction of sensors and wireless charging has broadened the application scenarios of LM-CNT-PEDOT:PSS. This method is simple to operate, fast to process, and easy to prepare and process on a large scale.
[0005] The objectives of the present invention are achieved through the following technical solutions.
[0006] A method for preparing a multi-fold mechanically enhanced self-healing supercapacitor, the method comprising the following steps:
[0007] (1) Dispersing carbon nanotube powder (CNT) in a pre-prepared solvent and stirring for 30 to 60 minutes to obtain a suspension.
[0008] The mass of the CNT in this step is 3 g, and the pre-configured solution is 130 ml of a mixed solution of sulfuric acid and nitric acid with a volume ratio of 3:1.
[0009] (2) The suspension obtained in step (1) is transferred to an oil bath for reaction, cooled to room temperature, diluted, centrifuged to obtain a precipitate, and then dispersed and dialyzed to obtain a carboxylated carbon nanotube solution.
[0010] The oil bath temperature in this step is 90° C. and the time is 2 to 3 hours.
[0011] (3) PEDOT:PSS and the carboxylated carbon nanotube solution obtained in step (2) are mixed and stirred for 30 to 90 minutes to obtain a CNT-PEDOT:PSS composite dispersion, and the solution is vacuum filtered to obtain a CNT-PEDOT:PSS composite film.
[0012] The concentration of the carboxylated CNT dispersion in this step is 5 mg / mL to 10 mg / mL, and PEDOT:PSS is a mixture of poly(3,4-ethylenedioxythiophene) (PEDOT) and polystyrene sulfonic acid (PSS), with a volume of 400 μL.
[0013] (4) The composite film obtained in step (3) is transferred to the pre-stretched nitrile substrate, and liquid metal (LM) is coated on the surface of the composite film. After releasing the tensile stress, a wrinkled LM-CNT-PEDOT:PSS composite film is obtained.
[0014] In this step, the liquid metal coating temperature is 90-120° C., the mass ratio of gallium to indium liquid metal is (10-40):70, and the thickness of the LM-CNT-PEDOT:PSS composite film is 20 μm to 60 μm.
[0015] (5) Polyvinyl alcohol (PVA) and phosphoric acid (H 3 PO 4 ) solution was dissolved in deionized water and stirred in an oil bath to obtain H 3 PO 4 -PVA gel electrolyte.
[0016] In this step, the molar mass of the polyvinyl alcohol is 1000-210000, the mass is 5 g, the volume of phosphoric acid is 3 mL, the volume of deionized water is 45 ml, the oil bath temperature is 90° C., and the stirring time is 2-3 hours.
[0017] (6) Under an argon atmosphere, the wrinkled LM-CNT-PEDOT:PSS film described in step (4) is processed into an interdigitated microelectrode by laser cutting technology, and then the H2O2 described in step (5) is dripped into the interdigitated microelectrode. 3 PO 4 -PVA gel electrolyte, the interdigitated microelectrodes are encapsulated by a thermoplastic film.
[0018] In this step, the interdigital electrodes have a length of 0.8 cm, a width of 100 μm to 900 μm, a gap of 50 μm to 200 μm, and are etched using a fiber laser with a power of 5W to 20W. The stimulation signal corresponding to the healing of the supercapacitor is temperature.
[0019] There is no time sequence restriction among the steps (1), (2) and (5).
[0020] Beneficial Effects
[0021] (1) The present invention utilizes the pre-stretching strategy and the rich oxygen-containing functional groups of carbon nanotubes to effectively reduce the surface potential energy of gallium-indium liquid metal, so that the CNT-PEDOT:PSS composite film is closely attached to the liquid metal. An oriented multi-fold LM-CNT-PEDOT:PSS film is constructed. The constructed LM-CNT-PEDOT:PSS film supercapacitor has excellent mechanical properties and shows good self-healing properties under temperature stimulation.
[0022] (2) The LM-CNT-PEDOT:PSS film described in the present invention can be arbitrarily integrated according to different energy and voltage requirements through the healing properties of liquid metal, expanding the application range of next-generation microelectronic devices. At the same time, the gallium-indium liquid metal coating further enhances its mechanical properties, enabling it to be used in the wearable field.
[0023] (3) The LM-CNT-PEDOT:PSS film described in the present invention shows excellent sensing signals under different strains and can be integrated with wireless charging to facilitate monitoring of physiological signals such as bending of fingers and arms, frowning, etc. This study provides a new strategy for the preparation of self-healing supercapacitors with multi-fold mechanical enhancements, realizing the functional integration of self-healing supercapacitors in wearables and sensors. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the processing process of the LM-CNT-PEDOT:PSS micro supercapacitor prepared in Examples 1 to 3
[0025] Figure 2 SEM and AFM images of the CNT-PEDOT:PSS side of the LM-CNT-PEDOT:PSS composite film prepared in Examples 1 to 3
[0026] Figure 3 SEM and AFM images of the LM side of the LM-CNT-PEDOT:PSS composite film prepared in Examples 1 to 3
[0027] Figure 4 SEM images of the cross-section of the LM-CNT-PEDOT:PSS composite film prepared in Examples 1 to 3
[0028] Figure 5 Flexible display electronic images of the LM-CNT-PEDOT:PSS composite films prepared in Examples 1 to 3
[0029] Figure 6 Electronic photos showing the stretchability of the LM-CNT-PEDOT:PSS composite films prepared in Examples 1 to 3
[0030] Figure 7 Performance pictures of LM-CNT-PEDOT:PSS micro-supercapacitors prepared in Examples 1 to 3
[0031] Figure 8 Schematic diagram of the self-healing mechanism of the LM-CNT-PEDOT:PSS composite film prepared in Examples 1 to 3
[0032] Fig. 9 Healing pictures of the LM-CNT-PEDOT:PSS composite films prepared in Examples 1 to 3
[0033] Fig.10 Healing pictures of the LM-LM healing method of the LM-CNT-PEDOT:PSS composite film prepared in Examples 1 to 3
[0034] Fig.11 The mechanical properties test diagram of the LM-CNT-PEDOT:PSS composite film prepared in Examples 1 to 3 after healing
[0035] Fig.12 The photos of the mechanical strength of the LM-CNT-PEDOT:PSS micro-supercapacitors prepared in Examples 1 to 3 after healing
[0036] Fig.13 Application pictures of LM-CNT-PEDOT:PSS micro-supercapacitors prepared in Examples 1 to 3
[0037] Fig.14 Signal detection pictures of LM-CNT-PEDOT:PSS composite thin film sensors prepared in Examples 1 to 3 DETAILED DESCRIPTION
[0038] The present invention is further described below by specific examples. Unless otherwise specified, the technical means used in the present invention are methods known to those skilled in the art. In addition, the present invention includes but is not limited to the following examples, and any equivalent replacement or local improvement carried out under the spirit and principle of the present invention will be deemed to be within the protection scope of the present invention.
[0039] In the following embodiments:
[0040] Scanning electron microscope (SEM): Japan REGULUS8100;
[0041] Element Energy Dispersive Spectrometer (EDS): American Apollo XLT SDD;
[0042] Atomic force microscope (AFM): Park NX10, South Korea;
[0043] X-ray diffractometer (XRD): Japan ULTIMALV;
[0044] Infrared spectrometer: Nicolet IS10 Fourier transform infrared spectrometer, frequency range 4000~400cm -1 .
[0045] Example 1
[0046] (1) Under ultrasonic stirring, 400 μL of PEDOT:PSS was added dropwise into 15 mL of CNT (5 mg / mL) solution and maintained for 1 h.
[0047] (2) Pour the above CNT-PEDOT:PSS solution into a vacuum filtration device to obtain a CNT-PEDOT:PSS composite film (thickness 15 μm).
[0048] (3) The above CNT-PEDOT:PSS composite film was transferred to a pre-stretched nitrile substrate.
[0049] (4) Gallium-indium liquid metal (mass ratio of 30:70) is melted at 90-120°C on a hot stage, and then the molten gallium-indium liquid metal is evenly covered on the CNT-PEDOT:PSS composite film by spin coating. Afterwards, the pre-stretched nitrile substrate is released, and the wrinkled LM-CNT-PEDOT:PSS composite film is separated from the nitrile substrate to obtain a LM-CNT-PEDOT:PSS film.
[0050] (5) Polyvinyl alcohol (PVA) and phosphoric acid (H 3 PO 4 ) solution was dissolved in deionized water and stirred in an oil bath to obtain H 3 PO 4 -PVA gel electrolyte.
[0051] (6) Using a fiber laser, the LM-CNT-PEDOT:PSS film was cut into interdigitated electrodes with a length of 0.8 cm, a width of 0.06 cm, and a gap of 0.02 cm. The H 3 PO 4 -PVA gel electrolyte, the interdigitated microelectrodes are encapsulated by a thermoplastic film.
[0052] Example 2
[0053] (1) Under ultrasonic stirring, 400 μL of PEDOT:PSS was added dropwise into 15 mL of CNT (10 mg / mL) solution and maintained for 1 h.
[0054] (2) Pour the above CNT-PEDOT:PSS solution into a vacuum filtration device to obtain a CNT-PEDOT:PSS composite film (thickness 30 μm).
[0055] (3) The above CNT-PEDOT:PSS composite film was transferred to a pre-stretched nitrile substrate.
[0056] (4) Gallium-indium liquid metal (mass ratio of 20:70) is melted at 90-120°C on a hot stage, and then the molten gallium-indium liquid metal is evenly covered on the CNT-PEDOT:PSS composite film by spin coating. Afterwards, the pre-stretched nitrile substrate is released, and the wrinkled LM-CNT-PEDOT:PSS composite film is separated from the nitrile substrate to obtain a LM-CNT-PEDOT:PSS film.
[0057] (5) Polyvinyl alcohol (PVA) and phosphoric acid (H 3 PO 4 ) solution was dissolved in deionized water and stirred in an oil bath to obtain H 3 PO 4 -PVA gel electrolyte.
[0058] (6) Using a fiber laser, the LM-CNT-PEDOT:PSS film was cut into interdigitated electrodes with a length of 0.8 cm, a width of 0.06 cm, and a gap of 0.02 cm. The H 3 PO 4 -PVA gel electrolyte, the interdigitated microelectrodes are encapsulated by a thermoplastic film.
[0059] Example 3
[0060] (1) Under ultrasonic stirring, 400 μL of PEDOT:PSS was added dropwise into 15 mL of CNT (5 mg / mL) solution and maintained for 1 h.
[0061] (2) Pour the above CNT-PEDOT:PSS solution into a vacuum filtration device to obtain a CNT-PEDOT:PSS composite film (thickness 15 μm).
[0062] (3) The above CNT-PEDOT:PSS composite film was transferred to a pre-stretched nitrile substrate.
[0063] (4) Gallium-indium liquid metal (mass ratio of 10:70) is melted at 90-120°C, and then the molten gallium-indium liquid metal is evenly covered on the CNT-PEDOT:PSS composite film by spin coating. Afterwards, the pre-stretched nitrile substrate is released, and the wrinkled LM-CNT-PEDOT:PSS composite film is separated from the nitrile substrate to obtain a LM-CNT-PEDOT:PSS film.
[0064] (5) Polyvinyl alcohol (PVA) and phosphoric acid (H 3 PO 4 ) solution was dissolved in deionized water and stirred in an oil bath to obtain H 3 PO 4 -PVA gel electrolyte.
[0065] (6) Using a fiber laser, the LM-CNT-PEDOT:PSS film was cut into interdigitated electrodes with a length of 0.8 cm, a width of 0.06 cm, and a gap of 0.02 cm. The H 3 PO 4 -PVA gel electrolyte, the interdigitated microelectrodes are encapsulated by a thermoplastic film.
[0066] In step (4) of Examples 1 to 3, the LM-CNT-PEDOT:PSS film can be attached to a cylindrical glass tube and can be bent without cracking. In addition, the LM-CNT-PEDOT:PSS film can be stretched in two-dimensional and three-dimensional directions without cracks. Good flexibility and mechanical properties are demonstrated, such as Figure 5 , Figure 6 shown.
[0067] In step (4) of Examples 1 to 3, the overall thickness of the LM-CNT-PEDOT:PSS film is about 50 μm, the LM coating is tightly fixed on the CNT-PEDOT:PSS surface, and there is no crack at the interface between LM and CNT-PEDOT:PSS, which proves good bonding. Figure 4 shown.
[0068] according to Figure 2 and Figure 3 It can be seen that the upper and lower surfaces of the LM-CNT-PEDOT:PSS film described in step (4) of Examples 1 to 3 show different degrees of roughness. The maximum peak height of the CNT-PEDOT:PSS surface is about 267.1 nm, which is about 3 times that of the lower surface (98.9 nm), and has an oriented wrinkled structure, which can provide good stretchability and a larger contact reaction area for supercapacitors.
[0069] according to Figure 8 , Fig. 9 and Fig.10 It can be seen that the LM-CNT-PEDOT:PSS film described in step (4) of Examples 1 to 3 has good healing properties, which is attributed to the metallic bonds between LM and LM and the covalent bonds between LM and CNT-PEDOT:PSS.
[0070] The LM-CNT-PEDOT:PSS described in step (4) of Examples 1 to 3 was assembled into a microcapacitor and the electrochemical performance was tested. Figure 7 As shown, the micro-supercapacitor has good electrochemical performance, and the capacity retention rate is 85.09% after 10,000 cycles.
[0071] The LM-CNT-PEDOT:PSS film prepared in step (4) of Examples 1 to 3 has good healing properties. In addition, the repair of the liquid metal enhances the mechanical strength of the LM-CNT-PEDOT:PSS film. Fig.11 .
[0072] The LM-CNT-PEDOT:PSS micro-supercapacitor prepared in step (6) of Examples 1 to 3 has good healing properties. The cut LM-CNT-PEDOT:PSS micro-supercapacitor can be repaired at high temperature. No signs of healing were observed on the healed LM-CNT-PEDOT:PSS micro-supercapacitor. In addition, the liquid metal repair enhanced the mechanical strength of the LM-CNT-PEDOT:PSS micro-supercapacitor. The repaired LM-CNT-PEDOT:PSS micro-supercapacitor can withstand a weight of more than 100 grams, see Fig.12 .
[0073] The LM-CNT-PEDOT:PSS micro-supercapacitor prepared in step (6) of Examples 1 to 3 has good practical application value. It can be used for device energy supply, see Fig.13 .
[0074] The LM-CNT-PEDOT:PSS film prepared in step (4) of Examples 1 to 3 shows excellent sensing signals under different strains and can be integrated with wireless charging to facilitate monitoring of physiological signals such as bending of fingers and arms, frowning, etc. Fig.14 .
[0075] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a multi-fold mechanically enhanced self-healing supercapacitor, the method comprising the following steps: (1) Dispersing carbon nanotube powder (CNT) in a pre-prepared solvent and stirring for 30 to 60 minutes to obtain a suspension. (2) The suspension obtained in step (1) is transferred to an oil bath for reaction, cooled to room temperature, diluted, centrifuged to obtain a precipitate, and then dispersed and dialyzed to obtain a carboxylated carbon nanotube solution. (3) PEDOT:PSS and the carboxylated carbon nanotube solution obtained in step (2) are mixed and stirred for 30 to 90 minutes to obtain a CNT-PEDOT:PSS composite dispersion, and the solution is vacuum filtered to obtain a CNT-PEDOT:PSS composite film. (4) The composite film obtained in step (3) is transferred to the pre-stretched nitrile substrate, and liquid metal (LM) is coated on the surface of the composite film. After releasing the tensile stress, a wrinkled LM-CNT-PEDOT:PSS composite film is obtained. (5) Polyvinyl alcohol (PVA) and phosphoric acid (H3PO4) solution are dissolved in deionized water and stirred in an oil bath to obtain H3PO4-PVA gel electrolyte. (6) Under an argon atmosphere, the wrinkled LM-CNT-PEDOT:PSS film described in step (4) is processed into an interdigitated microelectrode using a laser cutting technique, and then the H3PO4-PVA gel electrolyte described in step (5) is dripped into the interdigitated microelectrode, and the interdigitated microelectrode is encapsulated using a thermoplastic film. There is no time sequence restriction among the steps (1), (2) and (5).
2. The method for preparing a multi-fold mechanically enhanced self-healing supercapacitor according to claim 1, characterized in that The carboxylated carbon nanotubes are prepared according to the following method: (a) 3 g of CNTs were dispersed in 130 ml of a pre-prepared solution of a mixed solution of sulfuric acid and nitric acid in a volume ratio of 3:1, and stirred for 30 to 60 minutes to obtain a suspension. (b) The suspension obtained in step (a) is transferred to a 90° C. oil bath for reaction for 2 to 3 hours, cooled to room temperature, and the mixed solution is diluted and centrifuged to obtain a precipitate, which is then dispersed and dialyzed to obtain a carboxylated carbon nanotube solution.
3. The method for preparing a multi-fold mechanically enhanced self-healing supercapacitor according to claim 1, characterized in that The concentration of the carboxylated CNT dispersion in step (3) is 5 mg / mL to 10 mg / mL, and PEDOT:PSS is a mixture of poly(3,4-ethylenedioxythiophene) (PEDOT) and polystyrene sulfonic acid (PSS), with a volume of 400 μL.
4. The preparation method according to claim 1, characterized in that In the step (4), the coating temperature of the liquid metal is 90-120° C., the mass ratio of gallium to indium liquid metal is (10-40):70, and the thickness of the LM-CNT-PEDOT:PSS composite film is 20 μm to 60 μm.
5. The preparation method according to claim 1, characterized in that In the step (5), the molar mass of polyvinyl alcohol is 1000-210000, the mass is 5 g, the volume of phosphoric acid is 3 mL, the volume of deionized water is 45 ml, the oil bath temperature is 90° C., and the stirring time is 2-3 hours.
6. The preparation method according to claim 1, characterized in that In the step (6), the length of the interdigitated electrodes is 0.8 cm, the width is 100 μm to 900 μm, and the gap is 50 μm to 200 μm.
7. The preparation method according to claim 1, characterized in that In step (6), the stimulation signal corresponding to the healing of the supercapacitor is temperature.
8. The preparation method according to claim 1, characterized in that In the step (6), a fiber laser with a power of 5W to 20W is used for etching.