Preparation method of flexible hafnium oxide-based ferroelectric capacitor

Preparation of hafnium zirconium oxygen ferroelectric film on flexible mica substrates through low-temperature atomic layer deposition method and electron beam evaporation technology, solving the problems of high power consumption of traditional hardware and complex processes, and achieving high integration, low energy consumption and environmental protection Flexible hafnium oxide-based ferroelectric capacitors are prepared, with excellent ferroelectric properties and mechanical flexibility.

CN119008272APending Publication Date: 2024-11-22XIANGTAN UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411255457.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional computing hardware faces the problems of high power consumption and storage mismatch when processing big data, and the preparation process of traditional flexible electronic devices is complex and not environmentally friendly, making it difficult to meet the needs of high integration and low energy consumption in the future.

Method used

A low-temperature atomic layer deposition method was used to prepare hafnium zirconium oxygen ferroelectric film on a flexible mica substrate, and the bottom electrode and the top electrode were prepared by electron beam evaporation. Combined with rapid annealing heat treatment, the process was simplified and the film density and flexibility were improved.

Benefits of technology

It realizes a flexible hafnium oxide-based ferroelectric capacitor with low temperature preparation, simple process, environmental protection, dense film and superior performance, with high integration and good ferroelectric properties, and maintains good performance especially in bending conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005033910990000011
    Figure HDA0005033910990000011
  • Figure HDA0005033910990000012
    Figure HDA0005033910990000012
  • Figure HDA0005033910990000021
    Figure HDA0005033910990000021
Patent Text Reader

Abstract

The invention relates to the field of ferroelectric capacitors, and discloses a preparation method of a flexible hafnium oxide-based ferroelectric capacitor. The method comprises the following steps: firstly, preparing a platinum or tungsten bottom electrode on a flexible mica sheet by adopting electron beam evaporation; depositing a zirconium-doped hafnium oxide ferroelectric film on the platinum or tungsten bottom electrode at a low temperature by adopting an atomic layer deposition method; finally, preparing tungsten as a top electrode by electron beam evaporation; and carrying out rapid thermal annealing treatment on the thin film to obtain the target flexible hafnium oxide-based ferroelectric capacitor with a sandwich structure. The flexible ferroelectric capacitor prepared by the invention does not need an additional functional layer, the preparation process is simplified, the remanent polarization of the hafnium-based ferroelectric film is remarkably improved, and the ferroelectric performance comparison of the device before and after bending shows that the flexible ferroelectric capacitor has excellent mechanical flexibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ferroelectric capacitors, and in particular to a method for preparing a flexible ferroelectric capacitor. Background Art

[0002] In recent years, the rapid development of technologies such as artificial intelligence, cloud computing, and 5G / 6G communications indicates that humanity is about to enter the era of the Internet of Everything. Since the post-Moore era, the demand for hardware computing power driven by deep learning-based artificial intelligence has grown exponentially. Traditional computing hardware based on the von Neumann architecture faces high power consumption challenges and a memory-computation mismatch when processing increasingly large and complex data sets. At the same time, the rise of artificial neural networks has driven the development of bio-inspired memory devices (such as artificial synapses), providing new opportunities to overcome the limitations of the post-Moore era.

[0003] As early as 2009, researchers proposed that the concept of bio-inspired memory devices is not necessarily limited to resistors but can be extended to capacitors and inductors. Capacitors, in particular, operate on the principle of capacitance, where information is transmitted as charge rather than current, resulting in lower static power consumption. Since the discovery of ferroelectricity in silicon-doped hafnium dioxide by German scientists in 2011, hafnium-based ferroelectric devices have been widely studied due to their high compatibility with CMOS technology, low energy consumption, and long-term data retention. Furthermore, flexible electronic devices such as wearable electronics and electronic skin have attracted considerable attention due to their superior portability and user-friendly interfaces compared to traditional silicon technology. Mica offers advantages over other flexible substrates, including a smooth surface, high thermal stability, high-temperature resistance, good chemical inertness, and excellent mechanical flexibility. Therefore, we chose mica as a substrate for fabricating flexible hafnium oxide-based ferroelectric capacitors, which combine superior ferroelectricity and high flexibility. Summary of the Invention

[0004] The present invention is directed to substrate materials and preparation technology for growing flexible hafnium oxide-based ferroelectric capacitors, and provides a preparation method for flexible hafnium oxide-based ferroelectric capacitors with low-temperature preparation, simple and environmentally friendly process, dense films and good performance.

[0005] The present invention provides a method for preparing a flexible hafnium oxide-based ferroelectric capacitor, comprising the following steps:

[0006] (1) Pt or W bottom electrodes were prepared on flexible mica substrates by electron beam evaporation;

[0007] (2) using atomic layer deposition to deposit a zirconium-doped hafnium oxide ferroelectric thin film on the Pt or W bottom electrode at low temperature;

[0008] (3) using electron beam evaporation to prepare metal W as a top electrode from the hafnium zirconium oxide ferroelectric thin film obtained in step (2);

[0009] (4) placing the film obtained in step (2) in an annealing furnace filled with an inert protective atmosphere for rapid annealing heat treatment, and taking out the sample after the annealing furnace cools to room temperature to obtain the target flexible hafnium oxide-based ferroelectric capacitor.

[0010] Furthermore, the hafnium source is tetrakis(dimethylamino)hafnium (TDMAHf), the zirconium source is tetrakis(dimethylamino)zirconium (TDMAZr), and water (H2O) is used as the oxygen source.

[0011] Furthermore, in step (1), the thickness of the Pt or W is 20 to 50 nanometers, and most preferably 20 nanometers.

[0012] Furthermore, in step (1), the flexible mica substrate is fluorophlogopite, and the preparation method is: smooth and crack-free fluorophlogopite sheets are selected and mechanically peeled to obtain mica sheets with a thickness of 30 to 50 microns.

[0013] Furthermore, in step (2), the atomic layer deposition to prepare the hafnium zirconium oxide ferroelectric thin film is performed by superlattice cyclic deposition, i.e., one cycle is to continuously deposit tetrakis(dimethylamino)hafnium and water twice, followed by continuously depositing tetrakis(dimethylamino)zirconium and water twice, and the total number of deposition cycles is 25, 30, and 35, respectively, and most preferably 30 cycles (thickness is about 10 nm).

[0014] Furthermore, in step (2), the purge time of the metal source and the water source is 40 seconds and 60 seconds, respectively. Sufficient purge time ensures the removal of reaction by-products during the deposition process.

[0015] Furthermore, in step (3), the electrode is a W electrode with a thickness of 20 nanometers.

[0016] Furthermore, in step (4), the inert protective atmosphere is nitrogen, and the specific annealing process is: heating from room temperature to 550°C at a heating rate of 3°C / s, keeping warm for 2 minutes, and then cooling to room temperature before taking out. During this process, the clamping stress of the top and bottom electrodes on the hafnium zirconium oxide film promotes the emergence of the ferroelectric phase.

[0017] The structure of the prepared flexible hafnium oxide-based ferroelectric capacitor is MFM, and its electrical properties are tested.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The hafnium zirconium oxide ferroelectric thin film prepared by ultra-low temperature atomic layer deposition (100°C) in the present invention is conducive to future high integration.

[0020] (2) The hafnium zirconium oxide ferroelectric film prepared by the present invention is dense and has a high remnant polarization.

[0021] (3) The present invention performs a thinning process on the mica substrate to ensure that the film will not crack when bent, so that the prepared ferroelectric film still has good ferroelectric properties when bent.

[0022] (4) The preparation process of the present invention is simple. No additional buffer layer and seed layer need to be added on the mica substrate. The metal electrode can be directly deposited, which simplifies the preparation process.

[0023] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The hafnium-zirconium ratio in Example 1 is 1:1, the film thickness is 10 nanometers, and the PV curves of the sample under unbent, compressed and stretched conditions respectively.

[0025] Figure 2 This is the CV curve of the sample in Example 1 with a hafnium-zirconium ratio of 1:1 and a film thickness of 10 nanometers.

[0026] Figure 3 This is the PV curve of the sample in Example 2 with a hafnium-zirconium ratio of 1:1 and a film thickness of 10 nanometers. DETAILED DESCRIPTION

[0027] In order to make the process and purpose of the present invention clearer, we will provide a more detailed step-by-step description.

[0028] Example 1

[0029] In this embodiment, different metals are used as electrode materials, including the following steps:

[0030] (1) First, mechanically peel off the fluorphlogopite mica sheet to about 50 microns, take the flexible mica substrate, and then use electron beam evaporation to prepare a 20 nanometer Pt bottom electrode on the mica sheet. The background vacuum is 10 -4 Below Pa.

[0031] (2) Atomic layer deposition is used to deposit a hafnium zirconium oxide thin film on the above-mentioned Pt bottom electrode at low temperature. A pre-deposition is performed before the formal deposition. The source pulses of hafnium, zirconium and water are observed in turn. After stabilization, the sample obtained in step (1) is placed in the chamber, and the deposition program is set (hafnium source: 0.3 seconds, water source: 0.05 seconds, hafnium source: 0.3 seconds, water source: 0.05 seconds, zirconium source: 0.3 seconds, water source: 0.05 seconds, zirconium source: 0.3 seconds, water source: 0.05 seconds), and after the vacuum is evacuated to below a certain degree, a carrier gas is introduced to start deposition, and finally a zirconium-doped hafnium oxide ferroelectric thin film is obtained.

[0032] (3) The thin film obtained in step (2) is used to prepare metal W as the top electrode by electron beam evaporation, wherein a mask plate is used for patterning. The patterned electrode is a circular electrode with a diameter of 200 microns, thereby obtaining an MFM structure capacitor.

[0033] (4) The capacitor obtained in step (3) was placed in an annealing furnace for rapid annealing heat treatment. The protective atmosphere was nitrogen. The specific annealing process was as follows: heating from room temperature to 550°C at a heating rate of 3°C / s, keeping the temperature for 2 minutes, and then cooling to room temperature before taking out. The ferroelectric performance was tested. The capacitance curve of the sample was measured to have obvious butterfly curve characteristics. When a voltage of 4V was applied to the sample, the residual polarization values ​​in the unbent, compressed and stretched states were 45.65μC / cm 2 , 41.41μC / cm 2 and 42.57 μC / cm 2 , the hysteresis loop and capacitance curve of the sample are as follows Figure 1 and Figure 2 shown.

[0034] Example 2

[0035] In this embodiment, the same metal is used as the electrode material, including the following steps:

[0036] (1) First, mechanically peel off the fluorine crystal mica sheet to about 50 microns, take the flexible mica substrate, and then use electron beam evaporation to prepare a 20 nm W bottom electrode on the mica sheet. The background vacuum is 10 -4 Below Pa.

[0037] (2) Atomic layer deposition is used to deposit a hafnium zirconium oxide thin film on the W bottom electrode at low temperature. A pre-deposition is performed before the formal deposition. The source pulses of hafnium, zirconium and water are observed in turn. After stabilization, the sample obtained in step (1) is placed in the chamber, and the deposition program is set (hafnium source: 0.3 seconds, water source: 0.05 seconds, hafnium source: 0.3 seconds, water source: 0.05 seconds, zirconium source: 0.3 seconds, water source: 0.05 seconds, zirconium source: 0.3 seconds, water source: 0.05 seconds), and the carrier gas is introduced after the vacuum is evacuated to below a certain degree to start deposition. Finally, a zirconium-doped hafnium oxide ferroelectric thin film is obtained.

[0038] (3) The thin film obtained in step (2) is used to prepare metal W as the top electrode by electron beam evaporation, wherein a mask plate is used for patterning. The patterned electrode is a circular electrode with a diameter of 200 microns, thereby obtaining an MFM structure capacitor.

[0039] (4) The capacitor obtained in step (3) was placed in an annealing furnace for rapid annealing heat treatment. The protective atmosphere was nitrogen. The specific annealing process was as follows: heating from room temperature to 550°C at a heating rate of 3°C / s, keeping the temperature for 2 minutes, and then cooling to room temperature before taking it out. The ferroelectric performance was tested, and the residual polarization value of the sample was measured to be 43.2μC / cm 2 The hysteresis loop of the sample is as follows Figure 3 shown.

Claims

1. A method for preparing a flexible hafnium oxide-based ferroelectric capacitor, characterized in that: The following steps are involved: (1) Platinum or tungsten bottom electrodes were prepared on flexible mica substrates by electron beam evaporation; (2) using an atomic layer deposition method to deposit a zirconium-doped hafnium oxide ferroelectric thin film on the above-mentioned platinum or tungsten bottom electrode at low temperature; (3) using the hafnium zirconium oxide ferroelectric thin film obtained in step (2) to prepare metal tungsten as a top electrode by electron beam evaporation; (4) placing the film obtained in step (3) in an annealing furnace filled with an inert protective atmosphere for rapid annealing heat treatment, and taking out the sample after the annealing furnace is cooled to room temperature to obtain the target flexible hafnium oxide-based ferroelectric capacitor.

2. The method for preparing a flexible hafnium oxide-based ferroelectric capacitor according to claim 1, characterized in that: In step (1), the flexible mica substrate is fluorpho-mica, and the preparation method is: fix a smooth and crack-free fluorpho-mica sheet on an operating table using double-sided tape; since mica has a layered structure, the mica sheet can be torn off layer by layer using pointed tweezers until a mica sheet with a thickness of 30 to 50 microns is obtained.

3. The method for preparing a flexible hafnium oxide-based ferroelectric capacitor according to claim 1, characterized in that: In step (1), the specific steps of preparing the platinum or tungsten electrode by electron beam evaporation include: preparing a layer of 20 to 50 nanometers of metal platinum or tungsten as a bottom electrode on a flexible mica sheet.

4. The method for preparing a flexible hafnium oxide-based ferroelectric capacitor according to claim 1, characterized in that: In step (2), the specific steps of preparing the hafnium zirconium oxide ferroelectric film by atomic layer deposition at low temperature include: pre-deposition is required before the formal deposition to obtain a relatively stable source pulse, and then the sample is placed in the chamber, the deposition temperature is 100°C, and the doping ratio of hafnium and zirconium can be changed by changing the source time of the hafnium source and the zirconium source, and the thickness of the hafnium zirconium oxide film can be changed by changing the total number of deposition cycles.

5. The method for preparing a flexible hafnium oxide-based ferroelectric capacitor according to claim 1, characterized in that: In step (3), the specific steps of preparing the tungsten electrode by electron beam evaporation include: using a mask plate to prepare a 20-nanometer layer of metal tungsten as a top electrode on the hafnium zirconium oxide film.

6. The method for preparing a flexible hafnium oxide-based ferroelectric capacitor according to claim 1, characterized in that: In step (4), the inert protective atmosphere is nitrogen, and the specific process of rapid thermal annealing of the hafnium zirconium oxide ferroelectric film is: heating from room temperature to 550°C at a heating rate of 3°C / s, keeping the temperature for 2 minutes, and then cooling to room temperature for removal.

Citation Information

Cited By

  • Flexible hafnium oxide-based ferroelectric memory capacitor integrated array and preparation method thereof

    CN120379280A