Packaging method for reducing plastic packaging thickness

By designing grooves on the etched frame and mounting the chip into the grooves, the risk of wafer cracking during the packaging process of wafers with a thickness of less than 100μm is solved, and the stability and yield of ultra-thin packaging are improved.

CN119008420APending Publication Date: 2024-11-22ZHENGZHOU XINGHANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411079513.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In existing packaging processes, wafers with a thickness of less than 100μm have an extremely high risk of cracking during the thinning, lamination, and dicing processes, making it impossible to guarantee product quality.

Method used

A groove slightly larger than the chip size is designed and etched on the etching frame. The chip is then mounted into the groove, and wire bonding and molding processes are performed to ensure that the chip portion is recessed into the groove, thereby enhancing the adhesion between the chip frame and the molding compound.

Benefits of technology

Without reducing the wafer thinning thickness, the package thickness was reduced, avoiding the risk of wafer cracking, improving the stability and yield of the package, and meeting the requirements of ultra-thin packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008420A_ABST
    Figure CN119008420A_ABST
Patent Text Reader

Abstract

The invention discloses a packaging method for reducing plastic packaging thickness, and belongs to the field of semiconductor integrated circuit packaging tests.The method comprises the steps that in the etching frame design and manufacturing stage, a groove slightly larger than a chip in size is etched in a chip frame, the chip is attached to the interior of the groove, then the procedures of routing, plastic packaging and the like are carried out, and packaging of the chip is completed; therefore, on the premise of not further reducing the thinning thickness of the wafer, due to the design of the groove, a part of the chip sinks into the groove, so that the thickness of the part exposed out of the plane of the chip frame is reduced, and the processing requirement of ultrathin packaging is met; by adopting the method, packaging processing of the ultrathin QFN / DFN can be completed under the condition that the thinning thickness of the wafer is not reduced, and the risk of cracking caused by the fact that the thickness of the chip is very thin is avoided; the method is simple in principle, convenient to implement and high in product percent of pass, and has good popularization and application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor integrated circuit packaging and testing, and in particular relates to a packaging method for reducing plastic packaging thickness. Background Art

[0002] In order to meet the requirements of thinner and lighter semiconductor devices, the thickness of electronic components is getting thinner and thinner, and the thickness of chips is also getting thinner and thinner. During the packaging process, the wafer is thinned and thinner, and there is a risk of wafer cracking during the thinning, film pasting, dicing and core loading processes.

[0003] There are currently two methods in the industry to reduce the risk of chipping: the first is the Taiko process, and the second is to first apply the dicing film and then peel off the thin film. The first method is to reduce the risk of chipping by not thinning the edge area of ​​the wafer. The Taiko process requires the purchase of special equipment, which is extremely expensive and costly, and cannot be promoted on a large scale. The second method is a commonly used operation method in the industry. The specific process is: (1) Use blue film to stick on the front of the wafer; (2) Use a thinning machine to thin the back of the wafer; (3) Use a chip mounter to mount the back of the thinned wafer; (4) Use a film peeling machine to remove the protective film on the front of the wafer to expose the front of the wafer; (5) Use a dicing machine to cut the wafer; (6) Mount the thinned chip on the etching frame. The second method can reduce the risk of chipping to a certain extent for wafers with a thinning thickness of 100μm-200μm, but for wafers that need to be thinned to 100μm or less, there is still a very large risk of chipping.

[0004] It can be seen from this that for wafers with a thickness of less than 100μm, using the existing packaging process, the risk of wafer cracking is very high due to the very thin thickness of the wafer, and the product quality cannot be guaranteed. Summary of the invention

[0005] The present invention aims to provide a packaging method for reducing the thickness of plastic packaging, so as to solve the technical problem that the wafer thickness is very thin, the risk of wafer cracking is very likely to occur, and the product quality cannot be guaranteed.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A packaging method for reducing plastic packaging thickness, comprising:

[0008] Step 1: The chip is subjected to film lamination, thinning and dicing processes in sequence to obtain the chip to be loaded;

[0009] Step 2: etching the chip frame to obtain a groove with a preset depth;

[0010] Step 3: Mount the chip to be loaded into the groove of the chip frame;

[0011] Step 4: Wire-bonding the chip mounted in the groove to the chip frame;

[0012] Step 5: The chip frame after wire bonding will be plastic-sealed.

[0013] Furthermore, in step 2, the preset depth of the groove has the following relationship with the chip thickness and the thickness required by the process:

[0014] Chip thickness = preset depth of groove + thickness required by process.

[0015] Furthermore, in step 1, the specific steps of film lamination, thinning and dicing the chip are as follows:

[0016] Use a film laminating machine to apply UV protective film on the front of the chip;

[0017] Use a thinning machine to thin the film-laminated chip to a preset thickness;

[0018] Use a dicing machine to dice the thinned chips to obtain chips to be loaded.

[0019] Furthermore, in step 1, before the thinned chip is diced, a UV irradiator is used to irradiate the front side of the chip after filming, and then the UV protective film on the front side of the chip after filming is peeled off.

[0020] Furthermore, before using a UV irradiator to irradiate the front side of the chip after filming, a film laminating machine is used to affix a dicing film to the back side of the chip after filming.

[0021] Furthermore, the chip with the UV protective film removed is baked and dried in sequence, and the baked and dried chip is mounted in the groove of the chip frame.

[0022] Furthermore, in step three, the specific steps of mounting the chip to be loaded into the groove of the chip frame include:

[0023] Use a die bonding machine to squeeze the conductive glue into the groove of the frame, and then mount the upper core chip onto the conductive glue in the groove of the frame.

[0024] Furthermore, in step 4, the specific steps of wire bonding the chip mounted in the groove to the chip frame include:

[0025] The chip mounted in the groove is bonded to the chip frame using a wire bonder and gold wire or palladium-plated copper wire.

[0026] Furthermore, in step 5, the specific steps of plastic encapsulating the chip frame after wire bonding include:

[0027] The chip frame is plastic-sealed using a plastic-sealing material and a plastic-sealing machine, so that the plastic-sealing material fills into the groove in the chip frame to enhance the bonding force between the plastic-sealing material and the chip frame.

[0028] Furthermore, the area of ​​the groove of the chip frame gradually increases from the top to the bottom.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The invention provides a packaging method for reducing the thickness of plastic packaging. In the etching frame design and manufacturing stage, the method etches a groove slightly larger than the chip size on the chip frame, mounts the chip inside the groove, and then performs processes such as wire bonding and plastic packaging to complete the chip packaging. In this way, under the premise of not further reducing the wafer thinning thickness, due to the design of the groove, a part of the chip sinks into the groove, thereby reducing the thickness of the exposed chip frame plane, thereby meeting the ultra-thin packaging processing requirements. The method can complete the packaging processing of ultra-thin QFN / DFN without reducing the wafer thinning thickness, thereby avoiding the risk of chip cracking due to the very thin chip thickness. The method is simple in principle, easy to implement, high in product qualification rate, and has good promotion and application value.

[0031] In addition, due to the design of the groove structure, the chip can maintain a certain thinning thickness, which can also avoid the risk of chip flipping due to the chip being too thin.

[0032] Preferably, in the present invention, the preset depth of the groove can be determined according to the chip thickness and the thickness required by the process, that is, the groove etching thickness can be determined to meet the thickness requirements of the process and improve the stability and reliability of the package.

[0033] Preferably, in the present invention, a film laminating machine is used to affix a UV protective film to the front side of the chip; a thinning machine is used to thin the chip after film laminating to a preset thickness; a dicing machine is used to dicing the thinned chip to obtain a chip to be loaded, thereby completing the film laminating, thinning and dicing processes in sequence, ensuring that the chip reaches the required size and state before packaging, laying the foundation for the subsequent packaging process, and improving the packaging efficiency and yield rate.

[0034] Preferably, in the present invention, a UV irradiator is used to irradiate and peel off the UV protective film before dicing to reduce the adhesion between the UV protective film and the front side of the chip, which helps to protect the chip from damage during the dicing process and improves the accuracy and efficiency of dicing.

[0035] Preferably, in the present invention, a dicing film is attached to the back of the chip to further protect the chip from damage during the dicing process, and also helps to improve the accuracy and stability of dicing.

[0036] Preferably, in the present invention, the chip with the UV protective film removed is baked and dried, so that residues on the chip surface can be removed, ensuring the cleanliness of the chip surface, thereby improving the reliability of subsequent mounting and wire bonding.

[0037] Preferably, in the present invention, a die bonding machine is used to squeeze the conductive glue into the frame groove, and the chip is mounted on the conductive glue, thereby ensuring a stable connection between the chip and the frame, and the conductive glue can also provide good electrical connection performance.

[0038] Preferably, in the present invention, a wire bonding machine and gold wires or palladium-plated copper wires are used for wire bonding, thereby achieving efficient and reliable electrical connection between the chip and the frame, and improving the overall performance of the packaged product.

[0039] Preferably, in the present invention, the chip frame is plastic-sealed using a plastic sealing material and a plastic sealing machine, and it is particularly pointed out that the plastic sealing material is filled into the groove. Since in existing products, the plastic sealing connection between the chip frame and the plastic sealing material is mostly a planar structure, the bonding strength of this structure is poor. By filling the plastic sealing material into the groove, the two are fully combined, which helps to enhance the bonding strength between the plastic sealing material and the chip frame and improve the sealing and stability of the package.

[0040] Preferably, in the present invention, the area of ​​the groove of the chip frame gradually increases from the top to the bottom, that is, the side wall and the bottom surface of the groove are inclined, and the angle between the two is preferably an acute angle; this design helps to better accommodate the chip and reduce the generation of bubbles and voids during the plastic packaging process, and further enhances the bonding strength between the plastic packaging material and the chip frame, thereby improving the yield and quality of the package. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 A schematic cross-sectional view of a conventional QFN / DFN etching frame after plastic packaging provided by an embodiment of the present invention;

[0042] Figure 2 A schematic cross-sectional view of a QFN / DFN etching frame encapsulated by the method provided in an embodiment of the present invention after plastic encapsulation;

[0043] Figure 3 A flow chart of a packaging method for reducing plastic packaging thickness provided by an embodiment of the present invention. DETAILED DESCRIPTION

[0044] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0045] It should be noted that when an element is referred to as being "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only embodiment.

[0046] Example 1

[0047] As mentioned in the background art, for wafers with a thickness of less than 100 μm, the existing packaging process is used. Since the wafer thickness is very thin, there is a risk of wafer cracking, and the product quality cannot be guaranteed.

[0048] like Figure 1 As shown, the thinned chip is mounted on the die pad of the etching frame (the chip carrier of the chip frame), the chip and the pins are connected using bonding wires, and then the chip is plastic-sealed. It can be seen that if the ultra-thin process requirements are met, the thickness of the chip needs to be controlled below 100μm. In this way, the chip is prone to cracking, disconnection and other risks due to being too thin, affecting the product qualification rate.

[0049] Figure 1 In the present invention, Die refers to a separate wafer area; Leadframe refers to the lead frame, that is, the etching frame (also called chip frame) in the present invention; Epoxy Molding Component refers to the plastic packaging material.

[0050] In order to solve the above problems, this embodiment provides a packaging method for reducing the thickness of the plastic package. This method optimizes the etching frame during the etching frame design and production stage to avoid the chipping problem caused by the pursuit of ultra-thin wafer thickness, improves the process window of thinning, dicing and chip loading, and provides a new solution to meet the requirements of thinning semiconductor devices. The specific ideas are as follows:

[0051] The thickness of the QFN / DFN etching frame (i.e., chip frame) is generally 0.2 or 0.15 mm, and the Die Pad is a flat silver-plated area. This method semi-etches a groove slightly larger than the chip size and of a certain depth on the Pad of the etching frame according to the size of the chip. The area around the groove is still a silver-plated area for easy wire bonding. When mounting the core, the chip is mounted in the groove area, followed by wire bonding, plastic sealing and other processes.

[0052] In order to better understand the packaging method for reducing the plastic packaging thickness provided in this embodiment, the following terms are explained:

[0053] QFN: The full name is Quad Flat No-lead Package, which means square flat no-lead packaging process;

[0054] DFN: The full name is Dual Flat No-Lead Package, which means a flat no-lead packaging process on both sides.

[0055] like Figure 3 As shown, this embodiment provides a packaging method for reducing the thickness of plastic packaging, which specifically includes the following steps:

[0056] Step 1: The chip is subjected to film lamination, thinning and dicing processes in sequence to obtain the chip to be loaded.

[0057] The specific operation steps are as follows:

[0058] Use a film laminating machine to apply UV protective film on the front of the chip;

[0059] Use a thinning machine to thin the film-laminated chip to a preset thickness;

[0060] Use a film laminating machine to attach a dicing film to the back of the wafer;

[0061] Use an oven to bake the wafer after thinning and film bonding;

[0062] Use a UV irradiator to irradiate the front of the chip after filming, and then peel off the UV protective film on the front of the chip after filming;

[0063] Use a dicing machine to dice the thinned chips to obtain chips to be loaded.

[0064] like Figure 2 As shown, step 2: etching the chip frame to obtain a groove with a preset depth. The groove of the chip frame gradually increases in area from the top to the bottom, and the overall size is slightly larger than the chip size.

[0065] In this embodiment, the preset depth of the groove has the following relationship with the chip thickness and the thickness required by the process:

[0066] Chip thickness = preset depth of groove + thickness required by process.

[0067] The chip thickness here refers to the wafer thickness of the bare chip after thinning and dicing, and the process required thickness refers to the minimum wafer thickness when thinning and dicing the core, which is usually 100μm.

[0068] Step 3: Mount the baked and dried chip into the groove of the chip frame.

[0069] Specifically, in this embodiment, a die bonding machine is used to squeeze the conductive glue into the groove of the frame, and then the chip after baking and spin drying is mounted on the conductive glue in the groove of the frame.

[0070] Step 4: Use a wire bonding machine and gold wire or palladium-plated copper wire to bond the chip mounted in the groove to the chip frame.

[0071] Step 5: Use a plastic encapsulation material and a plastic encapsulation machine to encapsulate the chip frame, so that the plastic encapsulation material fills into the groove in the chip frame to enhance the bonding force between the plastic encapsulation material and the chip frame, thereby completing the chip packaging.

[0072] This embodiment provides a packaging method for reducing the thickness of plastic packaging. The technical concept of the above specific steps is embodied in the following aspects:

[0073] First, as attached Figure 1 As shown, the Die Pad of a conventional etching frame is flat. When loading the core, the chip is attached to the etching frame, followed by processes such as wire bonding and plastic sealing. This method requires the wafer to be thinned to a very thin thickness.

[0074] As attached Figure 2 As shown, in the etching frame design and manufacturing stage of this embodiment, a groove slightly larger than the chip size is etched on the upper half of the Die Pad, the chip is mounted inside the groove, and then wire bonding, plastic sealing and other processes are carried out. This embodiment can complete the packaging processing of ultra-thin QFN / DFN without reducing the thickness of the wafer.

[0075] Second, QFN / DFN is often mounted on a PCB board, and the device will absorb moisture and heat during operation, and the etching frame and the plastic packaging material will separate, resulting in device scrapping. The groove designed in this embodiment can enhance the bonding force between the etching frame and the plastic packaging material, reduce the risk of delamination of the etching frame and the plastic packaging material, and product scrapping.

[0076] Third, when the die bonding machine is loading the core, the die bonding machine first squeezes the conductive glue onto the die pad, and then sticks the chip onto the conductive glue. The conductive glue serves to connect the etching frame and the chip. In this process, if the chip is too thin, the glue is very easy to flip over, and the glue overflows to the front of the chip, causing the chip to be scrapped. This embodiment increases the wafer thinning thickness and greatly reduces the risk of chip flipping.

[0077] Fourth, after the conductive glue is attached to the die pad, it is easy to spread, resulting in failure of subsequent bonding. This embodiment proposes a method of attaching the chip to the groove, so that the conductive glue can only spread in the groove, reducing the range of glue diffusion and greatly improving the process window and yield of the chip.

[0078] Fifth, the etching frame material is copper, and its mass density is much higher than that of the plastic packaging material and the chip. Compared with the conventional etching frame packaging, this method greatly reduces the mass of the plastic packaging device, meeting the requirement of lighter and lighter device mass.

[0079] Sixth, when designing the size and position of the groove, the chip size, the accuracy of the die bonding machine and the wiring of the bonding wire should be fully considered. The groove size should be at least 50μm larger than the chip size, but not too large, otherwise the etching solution may cause the edge of the die pad to separate from the etching frame during the etching frame production stage.

[0080] It can be seen that this embodiment provides a packaging method for reducing the thickness of the plastic package. By etching a groove on the etching frame DiePad, the requirements for thinning the device can be met while ensuring the thickness of the wafer is reduced.

[0081] Example 2

[0082] This embodiment provides a packaging method for reducing the thickness of plastic packaging, which is applied to QFN36L products, 5×5mm, 0.30mm thick ultra-thin packaging, and the specific steps are as follows:

[0083] Step 1: Use a film laminating machine to paste a UV protective film on the front of the wafer; in the present invention, the wafer refers to the wafer of the chip.

[0084] Step 2: Use a thinning machine to thin a 12-inch wafer with an initial wafer thickness of 889 μm and a chip size of 1.6 mm × 1.6 mm to 120 μm;

[0085] Step 3: Use a die mounter to attach a dicing film to the back of the thinned 12-inch wafer;

[0086] Step 4: Use a UV irradiator to irradiate the front side of the 12-inch wafer to reduce the bonding effect between the UV protective film and the front side of the wafer, and then manually peel off the UV protective film on the front side of the wafer;

[0087] Step 5: Place the 12-inch wafer with the backside dicing film in an oven for baking;

[0088] Step 6: Use a dicing machine to dice the 12-inch wafer;

[0089] Step 7: Use a spin dryer to spin dry the 12-inch wafer after dicing;

[0090] Step 8: Design and make an etching frame with a thickness of 0.15 mm and a groove depth of 0.11 mm;

[0091] Step 9: Use a die bonding machine to squeeze the conductive glue into the groove, and then mount the wafer (chip) onto the conductive glue on the etching frame;

[0092] Step 10: Use a wire bonding machine and a 20 μm diameter gold wire to connect the chip to the etching frame;

[0093] Step 11: Use a mold cap with a height of 0.15 mm to mold the etching frame.

[0094] Example 3

[0095] This embodiment provides a packaging method for reducing the thickness of plastic packaging, which is applied to QFN28L, 4×4 mm, 0.4 mm thick ultra-thin packaging. The specific steps are as follows:

[0096] Step 1: Use a film laminating machine to apply UV protective film on the front of the wafer;

[0097] Step 2: Use a thinning machine to thin a 12-inch wafer with an initial thickness of 776 μm and a chip size of 1.3 mm × 1.3 mm to 150 μm;

[0098] Step 3: Use a die mounter to attach a dicing film to the back of the thinned 12-inch wafer;

[0099] Step 4: Use a UV irradiator to irradiate the front side of the 12-inch wafer to reduce the bonding effect between the UV protective film and the front side of the wafer, and then manually peel off the UV protective film on the front side of the wafer;

[0100] Step 5: Place the 12-inch wafer with the backside dicing film in an oven for baking;

[0101] Step 6: Use a dicing machine to dice the 12-inch wafer;

[0102] Step 7: Use a spin dryer to spin dry the 12-inch wafer after dicing;

[0103] Step 8: Design and make an etching frame with a thickness of 0.20 mm and a groove depth of 0.1 mm;

[0104] Step 9: Use a die bonding machine to squeeze the conductive glue into the groove, and then mount the chip onto the conductive glue on the etching frame;

[0105] Step 10: Use a wire bonder and 25 μm diameter palladium-plated copper wire to connect the chip to the etching frame;

[0106] Step 11: Use a mold with a Mold Cap of 0.20 mm to plastic-encapsulate the etched frame.

[0107] In summary, this embodiment provides a packaging method for reducing the thickness of plastic packaging, which has the following advantages compared to the existing packaging process:

[0108] First, the chip is processed by filming, thinning, and dicing, and then mounted on a chip frame with a preset depth groove after etching. This packaging method significantly reduces the thickness of the plastic package, making the packaged product more compact, which is conducive to saving space and improving integration. At the same time, the preset depth of the groove is accurately set according to the chip thickness and the thickness required by the process, ensuring that the chip can be firmly embedded in the groove, which not only meets the precision requirements of the package, but also improves the reliability of the package. The use of this method can meet the thickness requirements of the ultra-thin packaging process on the basis of chip quality assurance. In the specific steps of filming, thinning, and dicing, the use of UV protective film and dicing film, as well as UV irradiation, baking and drying treatment are introduced to effectively protect the integrity of the chip during the processing process, reduce damage during the dicing process, and improve the chip yield. Conductive glue is used to mount the chip in the frame groove, and a wire bonding machine and high-quality wire are used for wire bonding, which ensures the stability and reliability of the electrical connection between the chip and the frame, and improves the overall performance of the packaged product. In the plastic encapsulation process, the plastic encapsulation material is used to fill the groove, which enhances the bonding force between the plastic encapsulation material and the chip frame, improves the sealing and stability of the package, and further ensures the quality and reliability of the packaged product. Finally, the design of the chip frame groove gradually increasing in area from top to bottom optimizes the package structure, helps reduce bubbles and voids in the plastic encapsulation process, and improves the yield and quality of the package. In summary, this method shows significant beneficial effects in reducing the thickness of the plastic encapsulation, improving the accuracy and reliability of the package, and optimizing the package structure.

[0109] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0110] The above are only preferred specific implementation modes of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and the disclosed concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

[0111] The further detailed description made in the disclosure cannot be used to determine that the specific implementation modes of the present invention are limited to these. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention determined by the submitted claims.

Claims

1. A packaging method for reducing the thickness of plastic packaging, It is characterized in that include: Step 1: The chip is subjected to film lamination, thinning and dicing processes in sequence to obtain the chip to be loaded; Step 2: etching the chip frame to obtain a groove with a preset depth; Step 3: Mount the chip to be loaded into the groove of the chip frame; Step 4: Wire-bonding the chip mounted in the groove to the chip frame; Step 5: The chip frame after wire bonding will be plastic-sealed.

2. A packaging method for reducing plastic packaging thickness according to claim 1, It is characterized in that In step 2, the preset depth of the groove has the following relationship with the chip thickness and the thickness required by the process: Chip thickness = preset depth of groove + thickness required by process.

3. A packaging method for reducing plastic packaging thickness according to claim 1, It is characterized in that In step 1, the specific steps of film lamination, thinning and dicing the chip are as follows: Use a film laminating machine to apply UV protective film on the front of the chip; Use a thinning machine to thin the film-laminated chip to a preset thickness; Use a dicing machine to dice the thinned chips to obtain chips to be loaded.

4. A packaging method for reducing plastic packaging thickness according to claim 3, It is characterized in that In step 1, before the thinned chip is diced, a UV irradiator is used to irradiate the front side of the chip after filming, and then the UV protective film on the front side of the chip after filming is peeled off.

5. A packaging method for reducing plastic packaging thickness according to claim 4, It is characterized in that Before using a UV irradiator to irradiate the front side of the chip after filming, a film laminating machine is used to affix a dicing film to the back side of the chip after filming.

6. A packaging method for reducing plastic packaging thickness according to claim 4, It is characterized in that The chip with the UV protective film removed is baked and dried in sequence, and the baked and dried chip is mounted in the groove of the chip frame.

7. A packaging method for reducing plastic packaging thickness according to claim 1, It is characterized in that In step 3, the specific steps of mounting the chip to be mounted into the groove of the chip frame include: Use a die bonding machine to squeeze the conductive glue into the groove of the frame, and then mount the upper core chip onto the conductive glue in the groove of the frame.

8. A packaging method for reducing plastic packaging thickness according to claim 1, It is characterized in that In step 4, the specific steps of wire bonding the chip mounted in the groove to the chip frame include: The chip mounted in the groove is bonded to the chip frame using a wire bonder and gold wire or palladium-plated copper wire.

9. A packaging method for reducing plastic packaging thickness according to claim 1, It is characterized in that In step 5, the specific steps of plastic encapsulating the chip frame after wire bonding include: The chip frame is plastic-sealed using a plastic-sealing material and a plastic-sealing machine, so that the plastic-sealing material fills into the groove in the chip frame to enhance the bonding force between the plastic-sealing material and the chip frame.

10. A packaging method for reducing plastic packaging thickness according to claim 1, It is characterized in that The groove of the chip frame gradually increases in area from the top to the bottom.