Aqueous zinc ion battery positive electrode material and preparation method and application thereof
By introducing cerium Ce doped VO2 into the positive electrode material of aqueous zinc ion battery, the problem of vanadium-based oxide structure prone to collapse and slow reaction kinetics is solved, the specific capacity and rate performance are improved, and better cycle performance is provided and stability, suitable for the development of aqueous zinc ion batteries.
Patent Information
- Application Number
- CN202411240701.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The positive electrode materials of aqueous zinc ion batteries have problems such as slow reaction kinetics, low specific capacity, poor cycle performance and rate performance in the optimization of electrochemical performance of aqueous zinc ion batteries, especially the problems of vanadium-based oxide structure prone to collapse and ion dissolution.
By introducing cerium Ce element doped VO2, a simple preparation method is used to form Ce doped VO2 material as the positive electrode material of aqueous zinc ion battery, and V2O5, Ce(NO3)3 and C2H2O4·2 (H2O) are used under specific ratios and conditions Reaction to form a rod-like structure Ce-VO2 material used to prepare high-performance positive electrode sheets.
It significantly improves the specific capacity, rate performance and long cycle performance of aqueous zinc ion batteries, provides more stable electrochemical performance, and is suitable for large-scale production.
Smart Images

Figure CN119008923A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of aqueous zinc ion batteries and relates to an aqueous zinc ion battery positive electrode material and a preparation method and application thereof. Background Art
[0002] With the continuous progress and development of human society, the consumption rate of traditional fossil energy is getting faster and faster. A global consensus has been reached on expanding and rationally utilizing sustainable clean energy such as wind energy and solar energy and establishing large-scale energy storage systems. In recent years, aqueous zinc-ion batteries have attracted more and more attention due to their advantages such as low cost, low flammability, non-toxicity, and high theoretical solubility. The research on battery systems in aqueous zinc-ion batteries is still in its early stages. The current focus is on designing high-performance cathode materials with high specific capacity and long cycle life. However, the optimization of the electrochemical performance of cathode materials for aqueous zinc-ion batteries still faces some challenges, mainly because zinc ions are divalent ions, which will produce strong electrostatic interactions with the matrix material, resulting in slow electrochemical reaction kinetics, low specific capacity, and poor cycle performance and rate performance. Therefore, the design and development of high-performance cathode materials is very necessary. Among many cathode materials, vanadium-based oxides have the advantages of low cost and simple preparation methods, and their application in aqueous zinc-ion batteries shows great potential. However, when vanadium-based oxides are used as positive electrode materials for aqueous zinc-ion batteries, there are problems such as easy structural collapse, easy dissolution of ions during the cycle, and slow reaction kinetics. The direct result is that the battery charging and discharging process is unstable, and the rate and cycle performance are poor.
[0003] The present invention provides a novel vanadium-based oxide aqueous zinc ion battery positive electrode material and a preparation method thereof, and is applied to aqueous zinc ion batteries, achieving great improvements in capacity, rate performance and long cycle performance. Summary of the invention
[0004] The invention provides a method for preparing an aqueous zinc ion battery positive electrode material to achieve the purpose of solving the above-mentioned problem.
[0005] A method for preparing a positive electrode material for an aqueous zinc ion battery, the specific steps are as follows: Weigh V2O5, Ce(NO3)3 and C2H2O4·2(H2O) into the lining of the reactor, add water and stir; The liner was moved into a stainless steel housing and then placed in an oven to continue the reaction; After the mixture cools down to room temperature naturally, take out the liner, pour off the supernatant, transfer the product at the bottom to a centrifuge tube, and centrifuge it 3 times with water; The sample after centrifugation is freeze-dried to obtain the positive electrode material of the aqueous zinc ion battery, and is stored in a small centrifuge tube.
[0006] Furthermore, in step (1), the mass ratio of V2O5, Ce(NO3)3 and C2H2O4·2(H2O) is 4:1:1-2, 15-20 times the amount of water is added, and a magnetic stirrer is used to stir for 1-2 hours.
[0007] Preferably, the masses of V2O5, Ce(NO3)3 and C2H2O4·2(H2O) are 0.6911 g, 0.1736 g and 1.008 g respectively, 35 mL of water is added, and the mixture is stirred with a magnetic stirrer for 1 h.
[0008] Furthermore, in step (2), the oven temperature is 180-220° C., and the reaction time is 15-20 h.
[0009] Preferably, the oven temperature is 200° C. and the reaction time is 18 h.
[0010] Furthermore, the positive electrode material of the aqueous zinc ion battery prepared by the above method has a rod-like structure.
[0011] The present invention also provides an application of an aqueous zinc ion battery positive electrode material. The aqueous zinc ion battery positive electrode material prepared by the above method is mixed with acetylene black and polyvinylidene fluoride, ground in an N-methyl-2-pyrrolidone solvent to form a slurry, and the obtained slurry is coated on a titanium foil and dried to obtain an aqueous zinc ion battery positive electrode sheet.
[0012] Furthermore, the mass ratio of the aqueous zinc ion battery positive electrode material, acetylene black, and polyvinylidene fluoride is 7:2:1.
[0013] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a method for preparing a novel vanadium-based oxide aqueous zinc ion battery positive electrode material, which is mainly through the introduction of cerium Ce element doping VO2. The method does not require complex steps and reaction equipment, has a simple process, is easy to operate, and is easy to mass produce. When the prepared Ce-doped VO2 material is used as a positive electrode material for an aqueous zinc ion battery, it exhibits better specific capacity, rate and long cycle performance under high current than non-Ce-doped VO2 material, providing new possibilities for the development of aqueous zinc ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0015] Figure 1This is a SEM image of the Ce-VO2 doped material synthesized in the example; Figure 2 XRD pattern of VO2 prepared in comparative example; Figure 3 XRD pattern of Ce-VO2 prepared in Example; Figure 4 It is the rate performance diagram under different current density; Figure 5 This is the cycle performance diagram at a current density of 5000 mA / g. DETAILED DESCRIPTION
[0016] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0017] Example A method for preparing a positive electrode material for an aqueous zinc ion battery, the specific steps are as follows: Weigh 0.6911 g of V2O5, 0.1736 g of Ce(NO3)3 and 1.008 g of C2H2O4·2(H2O) and pour them into the inner lining of the reactor, then add 35 mL of water, and then stir with a magnetic stirrer for 1 hour. After stirring; The liner was moved into a stainless steel shell and then placed in an oven to react at 200°C for 18 hours; After the liquid naturally cools to room temperature, take out the liner, discard the supernatant, transfer the product at the bottom to a centrifuge tube, and centrifuge it 3 times with water; After centrifugation, the sample is freeze-dried, taken out and stored in a small centrifuge tube.
[0018] like Figure 1 Shown is a SEM image of the Ce-VO2 doped material synthesized in the example. The material has a rod-like structure with a length of about 2.5 μm and a thickness of about 100 nm.
[0019] Comparative Example The difference from the embodiment is that Ce(NO3)3 is not added, and the VO2 material without Ce doping is prepared.
[0020] Test Case The positive electrode materials of aqueous zinc ion batteries prepared in the above-mentioned embodiments and comparative examples are respectively prepared into positive electrode sheets of aqueous zinc ion batteries, and then the aqueous zinc ion batteries are assembled, and the electrochemical performance of the assembled aqueous zinc ion batteries is tested.
[0021] (1) Preparation of electrodes: First, weigh 0.140 g, 0.040 g, and 0.020 g of the aqueous zinc ion battery positive electrode material prepared in the embodiment and comparative example, acetylene black, and polyvinylidene fluoride at a mass ratio of 7:2:1, and then grind them in N-methyl-2-pyrrolidone solvent for at least 30 minutes to form a slurry. Use a slicer to cut the titanium foil into discs with a diameter of 10 mm, and weigh the mass of the discs to be 0.00893 g. The prepared slurry is evenly coated on the titanium foil disc, and then transferred to an oven at 80°C for drying for about 6 hours. After drying, take it out and weigh the mass of the prepared electrode sheet. Calculate the mass of the active substance = (mass of the electrode sheet - 0.00893) × 0.7.
[0022] (2) Battery assembly: Use zinc foil as the negative electrode, glass fiber as the separator, and 3M zinc trifluoromethanesulfonate as the electrolyte. The battery assembly steps are as follows: Assemble in an air environment, and the assembly order is: positive battery case, positive electrode sheet, add a drop of electrolyte, glass fiber separator, add electrolyte to wet the separator, zinc foil, gasket, shrapnel, CR 2032 negative electrode case, and finally cover (note that the electrode sheet cannot touch the edge of the battery case). After assembly, use a battery packaging machine to package (note to wipe the squeezed electrolyte before and after each packaging).
[0023] (3) Electrochemical performance test: The electrochemical performance of the positive electrode material was tested by the button cell assembled as above. The rate performance and cycle performance were tested by constant current charge and discharge using a multi-channel battery test system. The constant current charge and discharge test curves were analyzed to evaluate electrochemical performance parameters such as rate performance and cycle performance. The current density applied for the rate performance test was 100mA / g, 200mA / g, 500mA / g, 1000mA / g, 2000mA / g, 5000mA / g, 10000mA / g, and 100mA / g in sequence, and then multiplied by the mass of the active material to set the current. The current density applied for the cycle performance test was 500mA / g, 1000mA / g, and 5000mA / g, respectively. The applied current was the mass of the active material of the electrode sheet in the battery sandwiched by the channel multiplied by the current density.
[0024] like Figure 2As shown in the figure, the rate performance tests of VO2 and Ce-VO2 aqueous zinc ion batteries carried out at current densities of 100 to 10000 mA / g show that the rate performance of Ce-VO2 is higher than that of pure phase VO2 at the same current density. The reversible specific capacities of Ce-VO2 samples at current densities of 100 mA / g, 200 mA / g, 500 mA / g, 1000 mA / g, 2000 mA / g, 5000 mA / g, and 10000 mA / g are 205.8 mAh / g, 153.5 mAh / g, 140.9 mAh / g, 132.7 mAh / g, 124.0 mAh / g, 106.7 mAh / g, 90.8 mAh / g, respectively. Back to 100 mA / g, the reversible specific capacity can still be maintained at 161.8mAh / g; at the same current density, the reversible specific capacity of VO2 samples are 180.9mAh / g, 133.4mAh / g, 96.1mAh / g, 78.7mAh / g, 65.6mAh / g, 50.3mAh / g, 38.1mAh / g, and the reversible specific capacity at 100mA / g can still be maintained at 127.5mAh / g. The results show that at the same current density, the reversible specific capacity of Ce-VO2 samples is higher than that of VO2 samples, and the rate performance after doping is better than that of pure phase VO2, indicating that the doped material Ce-VO2 can be used as a better electrode material.
[0025] like Figure 3 As shown in the figure, the long cycle performance test of VO2 and Ce-VO2 aqueous zinc ion batteries carried out at a high current density of 5000mA / g showed that the initial charge specific capacity of Ce-VO2 was 247mAh / g, and the initial discharge specific capacity was 243mAh / g; after 1400 cycles, the reversible capacity of the VO2 sample was 58mAh / g, while the reversible capacity of Ce-VO2 could still be maintained at 165mAh / g when it was cycled to 3000 cycles, indicating that at a current density of 5000 mA / g, Ce-VO2 exhibited better electrochemical properties, and doping with Ce effectively improved the retention of the reversible capacity of VO2 at high current density and the long cycle stability of the material.
[0026] In order to characterize the physical phase of the synthesized samples and explore whether the crystal structure of VO2 changes before and after doping, XRD tests were performed on the comparative VO2 and example Ce-VO2 synthetic materials. Figure 4 The X-ray diffraction pattern of VO2 prepared in the comparative example is shown. The sample has very obvious diffraction peaks, which correspond well to the peak positions of the standard card PDF#81-2392, and no other impurity peaks appear. Figure 5The X-ray diffraction pattern of the Ce-VO2 composite material prepared in the embodiment is shown. The sample also shows a very obvious diffraction peak position, which is consistent with the peak position of the standard card PDF#81-2392, and there are no other impurity peaks. By comparison, it can be seen that after Ce doping, the main diffraction peak of the composite material meets the peak position of the VO2 standard PDF card (PDF#81-2392), which indicates that the VO2 crystal structure in the synthetic material is not affected by Ce, and the crystal structure after doping has not changed, and can maintain its original crystal state.
[0027] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a positive electrode material for an aqueous zinc ion battery, characterized in that: The specific steps are: Weigh V2O5, Ce(NO3)3 and C2H2O4·2(H2O) and pour into the lining of the reactor, add water and stir; The liner was moved into a stainless steel housing and then placed in an oven to continue the reaction; After the mixture cools down to room temperature naturally, take out the liner, pour out the supernatant, transfer the product at the bottom to a centrifuge tube, and centrifuge it 3 times with water; The centrifuged sample is freeze-dried to obtain the positive electrode material of the aqueous zinc ion battery.
2. The method for preparing an aqueous zinc ion battery cathode material according to claim 1, wherein: In the step (1), the mass ratio of V2O5, Ce(NO3)3 and C2H2O4·2(H2O) is 4:1:1-2, 15-20 times the amount of water is added, and a magnetic stirrer is used to stir for 1-2 hours.
3. The method for preparing an aqueous zinc ion battery cathode material according to claim 1, wherein: In step (2), the oven temperature is 180-220° C. and the reaction time is 15-20 h.
4. The aqueous zinc ion battery positive electrode material prepared by the method according to any one of claims 1 to 3, characterized in that: The positive electrode material of the aqueous zinc ion battery is a rod-shaped structure.
5. The use of the aqueous zinc ion battery positive electrode material according to claim 4, characterized in that: The aqueous zinc ion battery positive electrode material, acetylene black and polyvinylidene fluoride are mixed, ground in N-methyl-2-pyrrolidone solvent to form slurry, and the obtained slurry is coated on titanium foil and dried to obtain an aqueous zinc ion battery positive electrode sheet.
6. The use of the aqueous zinc ion battery positive electrode material according to claim 5, characterized in that: The mass ratio of the aqueous zinc ion battery positive electrode material, acetylene black and polyvinylidene fluoride is 7:2:1.
Citation Information
Patent Citations
Magnesium ion doped VO2 (B) material as well as preparation method and application thereof
CN116230925A
Preparation method and application of rare earth ion intercalation vanadium oxide material
CN117105266A