Controllable preparation method of carbon-based negative electrode additive of lead-carbon battery

Through the complex precipitation coupled carbon thermal reduction strategy, the problems of complex and unstable preparation methods for carbon-based negative electrode additives in the leading carbon battery in the prior art are solved, and the uniform dispersion and close bonding of lead particles are achieved, which significantly improves the lead acid battery cycle life and electrochemical properties.

CN119008947AActive Publication Date: 2024-11-22JILIN UNIVERSITY

Patent Information

Application Number
CN202410926817.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-22
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The existing carbon-based negative electrode additive preparation methods for lead-carbon batteries have problems such as complex process, high cost, unstable performance and impurity pollution, making it difficult to achieve precise regulation and large-scale production of lead-carbon composite materials.

Method used

Using an efficient and stable complex precipitate coupled carbon thermal reduction strategy, the precipitate is prepared by mixing soluble lead salt, sodium acetate and carbon-based materials in purified water, adding organic acid solution, and then pyrolytic reduction in an inert atmosphere. Carbon-based negative electrode additive for lead-derived carbon batteries.

Benefits of technology

The uniform dispersion and close bonding of lead particles is achieved, the phenomenon of floating carbon is avoided, the repetition and stability of the material is improved, the hydrogen evolution reaction is inhibited, and the cycle life and electrochemical performance of lead-acid batteries are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008947A_ABST
    Figure CN119008947A_ABST
Patent Text Reader

Abstract

The invention discloses a controllable preparation method of a carbon-based negative electrode additive of a lead-carbon battery, which is a preparation method for realizing accurate regulation and control of lead and carbon through an efficient and stable complexing-precipitation coupling carbon thermal reduction strategy. Compared with other methods, the carbon-based negative electrode additive lead particles of the lead-carbon battery prepared by the method are uniformly anchored on the surface of the carbon material, the lead loading capacity is controllable, lead and carbon are tightly combined, impurities are not introduced, the high specific surface area and porosity of the carbon material can be reserved, and repeatability and stability are excellent. The preparation process of the method comprises the following steps: dispersing a complex precipitate formed by an organic acid and a soluble lead salt onto a carbon-based material in an aqueous solution, washing and drying a filtered substance, and pyrolyzing the filtered substance in a protective gas to obtain the lead-carbon battery negative electrode additive. According to the additive, the carbon floating phenomenon in the paste mixing process is avoided, the uniformity of a carbon material in a negative plate is improved, the hydrogen evolution reaction of the negative plate is inhibited, and the high-rate cycle life is prolonged. The method is simple to operate, controllable, low in cost and easy to realize large-scale preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a controllable preparation method of a carbon-based negative electrode additive for a lead-carbon battery, belonging to the technical field of lead-carbon batteries. Technical Background

[0002] In recent years, lead-carbon batteries, as an advanced lead-acid battery, not only have the advantages of lead-acid batteries such as safety, low cost and high recovery rate, but also optimize the microstructure of the negative electrode active material by adding various forms of carbon to the negative electrode, increase the porosity and electrode reaction kinetics of the negative electrode active material, alleviate the negative electrode sulfidation, and improve its competitiveness in hybrid vehicles, renewable energy storage, telecommunications backup power supply and other fields.

[0003] However, adding carbon to the negative electrode active material also brings some challenges. Carbon-based materials with lower hydrogen evolution overpotentials intensify the hydrogen evolution reaction, thereby reducing the capacitance contribution of the carbon-based materials and the coulombic efficiency of the battery, resulting in water loss in the electrolyte. As the cycle progresses, it will also destroy the electrode structure and induce failure mechanisms such as negative electrode expansion. In addition, due to the differences in physical and chemical properties between lead and carbon, carbon materials are often unevenly distributed in the negative electrode and the lead-carbon binding force is weak, and even carbon floating occurs. In the long run, the cycle life of lead-carbon batteries has not been well demonstrated. In order to simultaneously achieve the purpose of inhibiting hydrogen evolution at the negative electrode of lead-carbon batteries and alleviating sulfation, an effective solution is to prepare lead-carbon composite materials as negative electrode additives for lead-carbon batteries.

[0004] Up to now, the mainstream preparation methods of lead-carbon composite materials include electrodeposition, solid-phase ball milling, liquid-phase impregnation deposition precipitation, organic complex lead pyrolysis, etc. Chinese patent CN 102074702 A uses an electrodeposition method to deposit lead particles on activated carbon, but lead particles can only be deposited on the surface of the carbon coating, and the process of scraping from the motherboard for crushing will also destroy the structure of the composite material, and the electrodeposition uses a relatively expensive but non-conductive binder (such as polyvinylidene fluoride), which reduces the performance of the composite material and increases the preparation cost. CN 102945951 A ball-mills activated carbon and an organic carbon source together, and the mixture is granulated by spray drying, followed by pyrolysis and carbonization. The activated carbon agglomerates after pyrolysis are exposed to lead vapor for lead plating, and the lead content is controlled by controlling the time. This method is complex and inevitably has the risk of lead pollution and lead poisoning. CN103035895 A mixes an organic carbon source and lead powder in proportion and ball-mills them, then places them in a tubular furnace for carbonization, and then alternately washes them with an organic solvent and deionized water to obtain a carbon-coated lead powder composite material. CN 108899492 A mixes solid lead salt, solid strong base and carbon material by ball milling, so that the raw materials react chemically under the action of mechanical force to generate lead-carbon composite material. The material prepared by the solid phase ball milling method has low purity, uneven particle size distribution, large friction loss between the grinding body and the machine body, and will pollute the product. CN 109860531A uses carbon oxide to impregnate and adsorb lead ions dispersed by surfactant, and then obtains nano lead-carbon composite material by carbon thermal reduction. The prepared composite material has uneven lead particle distribution and uncontrollable lead loading, and poor repeatability. CN 110137452A and CN 103035894 A use a deposition precipitation method to deposit lead hydroxide or lead carbonate on a carbon material and pyrolyze to form a lead-carbon composite material. Although the lead content can be controlled, there are problems such as the need for precise pH control, poor reproducibility and uniformity, and the weak combination of lead and carbon carrier, which affects the overall performance of the material. CN104505511 A uses an organic complex of lead as a precursor, and calcines and pyrolyzes it at 200°C to 1000°C in an oxidizing atmosphere or an inert protective atmosphere. The carbon-containing precursor generates an amorphous carbon skeleton, and the lead salt decomposes or reduces to lead / lead oxide nanoparticles, which are firmly embedded in the carbon matrix to form a stable and efficient lead-carbon composite structure. However, the lead-carbon composite material synthesized by this method has too small a specific surface area and capacitance, and has limited improvement on the charge acceptance of the lead-carbon battery and the electrochemical active area of ​​the negative electrode active material. CN 105990578 A uses alginate complexed lead ions as a precursor, and carbonizes at low temperature to prepare active materials for lead-carbon battery electrodes. Due to its large molecular structure, lead alginate is more difficult to decompose, and a large amount of amorphous carbon and lead oxide are easily generated during the carbonization process, showing low conductivity, thereby affecting the electrochemical properties of the final product.It can be seen that the current preparation methods are not economically feasible for large-scale production, or because of the complex process, lengthy process, easy mixing of impurities, unstable performance, seriously affecting large-scale production. In this sense, it is urgent to develop a more concise, accurate and controllable preparation process to overcome this technical difficulty. Summary of the invention

[0005] The technical problem to be solved by the present invention is: to overcome the deficiencies in the prior art and provide a controllable preparation method for a carbon-based negative electrode additive for a lead-carbon battery, thereby achieving precise control of lead and carbon through an efficient and stable complex precipitation coupled carbon thermal reduction strategy.

[0006] In order to solve the technical problem, the technical solution adopted by the present invention is:

[0007] A controllable preparation method of a carbon-based negative electrode additive for a lead-carbon battery is provided, the method comprising the following steps:

[0008] 1) Mixing soluble lead salt, sodium acetate and carbon-based material in pure water to obtain a mixed solution A; the concentration of soluble lead salt in the mixed solution A is 0.01 mol L -1 ~0.10mol L -1 , the concentration of sodium acetate is 0.05 mol L -1 ~0.10molL -1 , the concentration of carbon-based materials was 0.2 g mL -1 ~1.0g mL -1 , sodium acetate is added to maintain pH stability and provide buffering function;

[0009] The carbon-based material includes one or more of activated carbon, carbon black, expanded graphite, graphene, carbon nanotubes, and carbon fibers, with a specific surface area of ​​20 m 2 g -1 ~2000m 2 g -1 , its particle size D90 = 20nm ~ 150μm;

[0010] 2) Prepare the concentration to 0.01 mol L -1 ~0.10mol L -1 The organic acid is a combination of one or more organic acids that can react with lead ions to form a precipitate;

[0011] 3) Add 0.5 mL / min of the mixed solution A under continuous stirring. -1 ~5.0mL min -1 Solution B was added at a rate of 100 to allow the precipitated white precipitate to settle on the carbon-based material, and the precipitate was filtered after standing, and the filtrate was washed to obtain a mixture C;

[0012] 4) drying the mixture C to obtain a black blended powder D;

[0013] 5) The black blended powder D is placed in an atmosphere furnace, and pyrolyzed and reduced at a temperature of 400° C. to 700° C. for 1 h to 6 h in an inert gas atmosphere to obtain a carbon-based negative electrode additive for a lead-carbon battery.

[0014] As a preferred embodiment of the present invention, the soluble lead salt in step 1) is one or more of lead nitrate and lead acetate.

[0015] As a preferred embodiment of the present invention, the organic acid in step 2) is citric acid, oxalic acid, tartaric acid, malic acid or amino acid.

[0016] As a preferred embodiment of the present invention, in step 3), the molar ratio of the soluble lead salt in the mixed solution A to the organic acid in the solution B is 1:1.

[0017] As a preferred embodiment of the present invention, the washing solution in step 3) is pure water or ethanol.

[0018] As a preferred embodiment of the present invention, the drying temperature in step 4) is 60° C. to 100° C., and the drying time is 4 h to 12 h.

[0019] As a preferred embodiment of the present invention, the inert gas flow rate in step 5) is 50-200 mL min -1 The heating rate of the atmosphere furnace is 2~5℃ min -1 .

[0020] As a preferred embodiment of the present invention, the inert gas in step 5) is one of nitrogen, argon and a hydrogen-argon mixture.

[0021] The lead loading amount of the carbon-based negative electrode additive for lead-carbon batteries prepared by the above method is 5.0wt.% to 50.0wt.%.

[0022] The present invention further provides an application method of the lead-carbon battery carbon-based negative electrode additive obtained by the present invention, wherein the prepared lead-carbon battery carbon-based negative electrode additive is added to the negative electrode lead paste according to a weight ratio, wherein the lead-carbon battery carbon-based negative electrode additive: lead powder is (0.2-5):100.

[0023] Beneficial effects of the present invention:

[0024] 1. Compared with the prior art, the complex precipitation method of the present invention has the characteristics of both the impregnation precipitation method (preparation with controllable lead content) and the organic complex lead pyrolysis method (repeatability and stability). The prepared carbon-based negative electrode additive for lead-carbon batteries has lead particles evenly dispersed on the carbon skeleton and the lead and the carbon skeleton are tightly bound by chemical bonds, which can achieve controllable preparation of lead loading without introducing impurities, and can retain the high specific surface area and porosity of the carbon material, with excellent repeatability and stability.

[0025] 2. The additive avoids the carbon floating phenomenon during the mixing process with the paste, improves the uniformity of the carbon material in the negative electrode plate, inhibits the hydrogen evolution reaction of the negative electrode plate, and increases the high-rate cycle life.

[0026] 3. The present invention is simple to operate, controllable, low-cost, and easy to achieve large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a scanning electron microscope (SEM) photograph of the Pb / RHAC-10 sample prepared in the present invention.

[0028] Figure 2 This is a scanning electron microscope (SEM) photograph of the Pb / RHAC-20 sample prepared in the present invention.

[0029] Figure 3 This is a scanning electron microscope (SEM) photograph of the Pb / RHAC-30 sample prepared in the present invention.

[0030] Figure 4 This is a high-resolution transmission electron microscope (HRTEM) photograph of the Pb / RHAC-20 sample prepared in the present invention.

[0031] Figure 5 It is a schematic diagram comparing the linear sweep voltammetry curves of the negative plates of Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2.

[0032] Figure 6 It is a schematic diagram comparing the high rate partial state of charge (HRPSoC) cycle life of the negative plates of Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described below in conjunction with the accompanying drawings and implementation cases.

[0034] Embodiment 1:

[0035] 1) 10.20 g of (CH3COO)2Pb·3H2O, 4.40 g of CH3COONa and 50 g of rice husk activated carbon (RHAC) were added to 1200 mL of pure water and mixed to obtain solution A. 5.60 g of C6H8O7·H2O was dissolved in 300 mL of pure water to form solution B. Solution B was slowly added to solution A under constant stirring at a drop rate of 1.0 mL min -1 , so that the precipitated white precipitate is deposited on RHAC. After the solution B is added, it is allowed to stand for 15 minutes, filtered, and the filtrate is washed with pure water to obtain a mixture C. It is then dried in an oven at 100°C for 12 hours to obtain a black blended powder D. Finally, the black powder D is placed in an atmosphere furnace and pyrolyzed and reduced in a nitrogen atmosphere at 500°C for 1 hour with a gas flow rate of 50 mL min -1 , heating rate is 2℃min -1 , and obtained a carbon-based negative electrode additive for lead-carbon batteries, named Pb / RHAC-10.

[0036] 2) Lead powder (100wt.%, oxidation degree 78%), Pb / RHAC-10 (1.00wt.%), short fiber (0.13wt.%), BaSO4 (0.80wt.%), sodium lignin sulfonate (0.20wt.%), humic acid (0.20wt.%), pure water (11.50wt.%), sulfuric acid (8.80wt.%), specific gravity 1.41g cm -3 ), mixed and evenly coated on the lead-tin-calcium alloy grid, and after solidification and chemical formation, the lead-carbon battery negative electrode was obtained.

[0037] Embodiment 2:

[0038] 1) 23.00 g of (CH3COO)2Pb·3H2O, 9.90 g of CH3COONa and 50 g of RHAC were added to 1200 mL of pure water and mixed to obtain solution A. 12.7 g of C6H8O7·H2O was dissolved in 300 mL of pure water to form solution B. Solution B was slowly added to solution A under constant stirring at a drop rate of 1.0 mL min -1 , so that the precipitated white precipitate is deposited on RHAC. After the solution B is added, it is allowed to stand for 15 minutes, filtered, and the filtrate is washed with pure water to obtain a mixture C. It is then dried in an oven at 100°C for 12 hours to obtain a black blended powder D. Finally, the black powder D is placed in an atmosphere furnace and pyrolyzed and reduced in a nitrogen atmosphere at 500°C for 1 hour with a gas flow rate of 50 mL min -1 The heating rate is 2℃ min -1 , and obtained a carbon-based negative electrode additive for lead-carbon batteries, named Pb / RHAC-20.

[0039] 2) Lead powder (100wt.%, oxidation degree 78%), Pb / RHAC-20 (1.00wt.%), short fiber (0.13wt.%), BaSO4 (0.80wt.%), sodium lignin sulfonate (0.20wt.%), humic acid (0.20wt.%), pure water (11.50wt.%), sulfuric acid (8.80wt.%), specific gravity 1.41g cm -3 ), mixed and evenly coated on the lead-tin-calcium alloy grid, and after solidification and chemical formation, the lead-carbon battery negative electrode was obtained.

[0040] Embodiment 3:

[0041] 1) 39.40 g of (CH3COO)2Pb·3H2O, 17.00 g of CH3COONa and 50 g of RHAC were added to 1200 mL of pure water and mixed to obtain solution A. 21.80 g of C6H8O7·H2O was dissolved in 300 mL of pure water to form solution B. Solution B was slowly added to solution A under constant stirring at a rate of 1.0 mL min -1 , so that the precipitated white precipitate is deposited on RHAC. After the solution B is added, it is allowed to stand for 15 minutes, filtered, and the filtrate is washed with pure water to obtain a mixture C. Then it is dried in an oven at 100°C for 12 hours to obtain a black blended powder D. Finally, the black powder D is placed in an atmosphere furnace and pyrolyzed and reduced in a nitrogen atmosphere at 500°C for 1 hour, with a gas flow rate of 50 mL min -1 The heating rate is 2℃ min -1 , and obtained a carbon-based negative electrode additive for lead-carbon batteries, named Pb / RHAC-30.

[0042] 2) Lead powder (100wt.%, oxidation degree 78%), Pb / RHAC-30 (1.00wt.%), short fiber (0.13wt.%), BaSO4 (0.80wt.%), sodium lignin sulfonate (0.20wt.%), humic acid (0.20wt.%), pure water (11.50wt.%), sulfuric acid (8.80wt.%), specific gravity 1.41g cm -3 ), mixed and evenly coated on the lead-tin-calcium alloy grid, and after solidification and chemical formation, the lead-carbon battery negative electrode was obtained.

[0043] Comparative Example 1:

[0044] Lead powder (100wt.%, oxidation degree 78%), short fiber (0.13wt.%), BaSO4 (0.80wt.%), sodium lignin sulfonate (0.20wt.%), humic acid (0.20wt.%), pure water (11.50wt.%), sulfuric acid (8.80wt.%, specific gravity 1.41g cm -3), mixed and evenly coated on the lead-tin-calcium alloy grid, and after curing and chemical formation, the negative electrode of the lead-acid battery was obtained.

[0045] Comparative Example 2:

[0046] Lead powder (100wt.%, oxidation degree 78%), RHAC (1.00wt.%), short fiber (0.13wt.%), BaSO4 (0.80wt.%), sodium lignin sulfonate (0.20wt.%), humic acid (0.20wt.%), pure water (11.50wt.%), sulfuric acid (8.80wt.%), specific gravity 1.41g cm -3 ), mixed and evenly coated on the lead-tin-calcium alloy grid, and after solidification and chemical formation, the lead-carbon battery negative electrode was obtained.

[0047] Implementation effect description

[0048] Figures 1 to 3 The SEM images of Pb / RHAC-10, Pb / RHAC-20, and Pb / RHAC-30 show that the lead particles are uniformly anchored on the surface of the RHAC skeleton. The average particle size ranges of Pb / RHAC-10, Pb / RHAC-20, and Pb / RHAC-30 are 103.2±28.0nm, 114.1±25.1nm, and 136.7±31.6nm, respectively. As the lead loading increases, the lead particles become more and more dense and agglomerated to form larger particles.

[0049] Figure 4 The HRTEM image of Pb / RHAC-20 shows a crystal plane spacing of 0.286 nm, which corresponds to the (111) plane of the Pb particles, proving that the lead particles are anchored successfully. It is worth noting that Pb / RHAC-20 consists of two structures, lead particles and RHAC, which are continuous and have no obvious gaps at the interface. This observation indicates that the bond between the lead particles and RHAC is very tight, which is conducive to the transmission of electrons and ions, thereby improving the electrochemical performance of the composite material.

[0050] Figure 5 The figure is a schematic diagram for comparing the linear sweep voltammetry curves of the negative electrode plates prepared in Examples 1 to 3, Comparative Example 1 and Comparative Example 2. At a potential of -1.6 V, we compared the hydrogen evolution currents of different electrodes. The hydrogen evolution current of Comparative Example 1 without adding rice husk activated carbon is the smallest (-0.111 Acm -2 ), due to the low hydrogen evolution overpotential inherent in carbon materials, the hydrogen evolution current of comparative example 2 with direct addition of rice husk activated carbon is the largest (-0.299Acm -2), however, the hydrogen evolution current of the lead-carbon battery negative electrode of Examples 1-3 to which Pb / RHAC-10, Pb / RHAC-20 and Pb / RHAC-30 prepared by the present invention are added decreased by 18.4%, 37.5% and 47.5% respectively compared with that of Comparative Example 2, and the hydrogen evolution current of the negative electrode plate is weakened, proving that the carbon-based negative electrode additive prepared by the present invention can effectively inhibit hydrogen evolution and slow down the water loss of the battery.

[0051] Figure 6 The diagram is a comparison of the cycle life of the lead-carbon battery negative electrode of Examples 1-3, Comparative Example 1 and Comparative Example 2 under high rate partial charge conditions (HRPSoC). The corresponding HRPSoC cycle life of the negative electrode of Comparative Example 2, Example 1, Example 2, and Example 3 is increased by 2.9 times, 6 times, 10 times, and 7.8 times, respectively, compared with the negative electrode of Comparative Example 1. The carbon-based negative electrode additive prepared by the present invention can greatly improve the HRPSoC cycle life of the lead-acid battery, and can also significantly inhibit the hydrogen evolution of the lead-carbon battery negative electrode and alleviate the problems caused by irreversible sulfation.

[0052] It should be noted that the above embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the appended claims of the present application.

Claims

1. A controllable preparation method of a carbon-based negative electrode additive for a lead-carbon battery, characterized in that: The method comprises the following steps: 1) Mixing soluble lead salt, sodium acetate and carbon-based material in pure water to obtain a mixed solution A; the concentration of soluble lead salt in the mixed solution A is 0.01 mol L -1 ~0.10mol L -1 , the concentration of sodium acetate is 0.05 mol L -1 ~0.10mol L -1 , the concentration of carbon-based materials was 0.2 g mL -1 ~1.0g mL -1 . The carbon-based material includes one or more of activated carbon, carbon black, expanded graphite, graphene, carbon nanotubes, and carbon fibers, with a specific surface area of ​​20 m 2 g -1 ~2000m 2 g -1 , its particle size D90 = 20nm ~ 150μm; 2) Prepare the concentration to 0.01 mol L -1 ~0.10mol L -1 The organic acid is a combination of one or more organic acids that can react with lead ions to form a precipitate; 3) Add 0.5 mL / min of the mixed solution A under continuous stirring. -1 ~5.0mL min -1 Solution B was added at a rate of 100 to allow the precipitated white precipitate to settle on the carbon-based material, and the precipitate was filtered after standing, and the filtrate was washed to obtain a mixture C; 4) drying the mixture C to obtain a black blended powder D; 5) The black blended powder D is placed in an atmosphere furnace, and pyrolyzed and reduced at a temperature of 400° C. to 700° C. for 1 h to 6 h in an inert gas atmosphere to obtain a carbon-based negative electrode additive for a lead-carbon battery.

2. The controllable preparation method of the carbon-based negative electrode additive for lead-carbon batteries according to claim 1, characterized in that: The soluble lead salt described in step 1) is one or more of lead nitrate and lead acetate.

3. The controllable preparation method of the carbon-based negative electrode additive for lead-carbon batteries according to claim 1, characterized in that: The organic acid in step 2) is citric acid, oxalic acid, tartaric acid, malic acid or amino acid.

4. The controllable preparation method of the carbon-based negative electrode additive for lead-carbon batteries according to claim 1, characterized in that: In step 3), the molar ratio of the soluble lead salt in the mixed solution A to the organic acid in the solution B is 1:

1.

5. The controllable preparation method of the carbon-based negative electrode additive for lead-carbon batteries according to claim 1, characterized in that: The washing solution in step 3) is pure water or ethanol.

6. The controllable preparation method of the carbon-based negative electrode additive for lead-carbon batteries according to claim 1, characterized in that: The drying temperature in step 4) is 60° C. to 100° C., and the drying time is 4 h to 12 h.

7. The controllable preparation method of the carbon-based negative electrode additive for lead-carbon batteries according to claim 1, characterized in that: The inert gas flow rate in step 5) is 50-200 mL min -1 The heating rate of the atmosphere furnace is 2~5℃ min -1 .

8. The controllable preparation method of the carbon-based negative electrode additive for lead-carbon batteries according to claim 1, characterized in that: The inert gas described in step 5) is one of nitrogen, argon and hydrogen-argon mixed gas.

9. A carbon-based negative electrode additive for lead-carbon batteries prepared by the method according to any one of claims 1 to 8, characterized in that: The lead loading amount of the carbon-based negative electrode additive for lead-carbon batteries is 5.0 wt.% to 50.0 wt.%.

10. The use of the carbon-based negative electrode additive for lead-carbon batteries as claimed in claim 9, characterized in that: The prepared lead-carbon battery carbon-based negative electrode additive is added to the negative electrode lead paste according to a weight ratio, wherein the lead-carbon battery carbon-based negative electrode additive: lead powder is (0.2-5):100.

Citation Information

Patent Citations

  • Preparation method of carbon-based composite material for cathode of lead-carbon battery

    CN107579240A

  • Nano lead / carbon composite material and preparation method thereof

    CN108134092A

  • Carbon additive, preparation method and application thereof

    CN113036126A

  • Preparation method of additive for effectively inhibiting irreversible sulfation of negative electrode

    CN117352739A

  • Negative electrode active material for lead storage battery and pb / c battery, preparation method therefor, and lead storage battery and pb / c battery comprising negative electrode active material

    US20230054947A1

Cited By

  • Preparation method of composite additive for lead-carbon battery

    CN122117919A

  • A method for preparing a composite additive for lead-carbon batteries

    CN122117919B