Proton exchange membrane doped and modified by double inorganic fillers

By doping CeO2, SiO2, Al2O3 and carbon nanotubes in the proton exchange membrane, combined with precise process steps, the stability of traditional membranes in high temperature and extreme environments is solved, and mechanical, electrical conductivity and chemical properties are improved, which is suitable for high efficiency Fuel cell applications.

CN119009040AActive Publication Date: 2024-11-22山西国润储能科技有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410656832.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-11-22
Estimated Expiration
2044-05-24

AI Technical Summary

Technical Problem

Traditional proton exchange membranes have mechanical stability, cost and operating temperature limitations under high temperature, high humidity or chemical extreme conditions, resulting in performance attenuation and reduced efficiency.

Method used

The modified proton exchange membrane is adopted with a dual inorganic filler doping. By anchoring CeO2, SiO2 and Al2O3 nanoparticles in the Nafion composite membrane matrix, and adding carbon nanotubes, combining precise process steps and temperature control, the membrane's mechanical and mechanical Thermal and chemical stability, as well as electrical conductivity.

Benefits of technology

It significantly improves the hardness, compressive resistance, conductivity and chemical stability of the membrane, extends the service life, improves the output efficiency and environmental adaptability of the fuel cell, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009040A_ABST
    Figure CN119009040A_ABST
Patent Text Reader

Abstract

The invention relates to the field of fuel cells, and discloses a dual inorganic filler doped and modified proton exchange membrane, which comprises a Nafion composite membrane matrix, ceO2 anchored on the amine functionalized cellulose nanofibers, wherein the CeO2 accounts for 2-5% of the total mass of the composite membrane; siO2 nano particles are added, wherein the SiO2 nano particles account for 0.5%-2% of the total mass of the composite film; al2O3 nano particles are added, wherein the Al2O3 nano particles account for 0.5%-2% of the total mass of the composite film. CeO2 is anchored on the amine functionalized cellulose nanofiber (CNF) and SiO2 and Al2O3 nanoparticles are added, so that the hardness and compression resistance of the composite membrane are remarkably improved, the service life of the composite membrane is prolonged, the reliability of the composite membrane is improved, meanwhile, the conductivity of the composite membrane is greatly enhanced by adding the carbon nanotubes (CNT), and the service life of the composite membrane is prolonged. The method is crucial for improving the output efficiency and the response speed of the fuel cell, and the overall energy conversion efficiency of the cell is directly influenced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fuel cells, in particular to a proton exchange membrane modified by doping with double inorganic fillers. Background Art

[0002] Fuel cell technology, as a clean energy conversion method, has attracted much attention due to its high energy efficiency and low environmental impact. In the fuel cell system, the proton exchange membrane (PEM) plays a vital role, acting as an electrolyte medium, allowing protons to pass through while blocking the flow of electrons. This process is directly related to the overall efficiency and energy output of the battery.

[0003] Traditional proton exchange membranes mostly use perfluorosulfonic acid polymer materials such as Nafion N, which have become industry standards due to their excellent chemical stability, good thermal stability and outstanding ion conductivity. However, these traditional materials still have certain limitations in their application under high temperature, high humidity or chemical extreme conditions:

[0004] Mechanical stability issues: During long-term operation or under high temperature and high pressure environments, polymer membranes may deform, resulting in performance degradation or even failure.

[0005] Cost issue: The manufacturing cost of materials such as Nafion N is high, which limits its popularity in large-scale commercial applications.

[0006] Operating temperature limit: The optimal operating temperature of traditional PEM generally does not exceed 80°C. Temperatures above this will cause the membrane hydration layer to lose stability and reduce proton transfer efficiency.

[0007] Therefore, the present invention proposes a proton exchange membrane modified by doping with dual inorganic fillers to solve the deficiencies of the prior art. Summary of the invention

[0008] In view of the shortcomings of the prior art, the present invention provides a proton exchange membrane doped and modified with dual inorganic fillers, which not only improves the mechanical and thermal stability of the traditional proton exchange membrane, but also significantly enhances its chemical stability and electrical conductivity.

[0009] To achieve the above objectives, the present invention is implemented by the following technical scheme: a proton exchange membrane doped and modified with dual inorganic fillers, comprising the following components:

[0010] Nafion composite membrane matrix;

[0011] CeO2 anchored on amine-functionalized cellulose nanofibers, wherein CeO2 accounts for 2% to 5% of the total mass of the composite membrane;

[0012] Adding SiO2 nanoparticles, wherein the SiO2 nanoparticles account for 0.5% to 2% of the total weight of the composite film;

[0013] Al2O3 nanoparticles are added, wherein the Al2O3 nanoparticles account for 0.5% to 2% of the total mass of the composite film.

[0014] Preferably, the amine-functionalized cellulose nanofibers account for 3% to 7% of the total mass of the Nafion composite membrane matrix.

[0015] Preferably, the particle sizes of CeO2, SiO2 and Al2O3 are all 5 to 20 nanometers.

[0016] Preferably, a dual inorganic filler doped and modified proton exchange membrane further comprises carbon nanotubes added in an amount of 0.3% to 3% to enhance the mechanical properties and electrical conductivity of the composite membrane.

[0017] Preferably, a proton exchange membrane doped and modified with dual inorganic fillers is characterized by comprising the following steps:

[0018] S1, mixing CeO2, SiO2 and Al2O3 nanoparticles with amine-functionalized cellulose nanofibers in a predetermined ratio to anchor these inorganic fillers on the surface of the amine-functionalized cellulose nanofibers;

[0019] S2, suspending the treated amine-functionalized cellulose nanofibers in Nafion solution at room temperature to form a uniform suspension;

[0020] S3, pouring the suspension into a flat film casting machine, and casting the film under the condition of controlling the temperature at 60° C. to 150° C.;

[0021] S4. The cast membrane was dried at room temperature for 24 hours and then heat treated in an oven at 80° C. for 2 hours to complete the curing and performance optimization of the membrane.

[0022] Preferably, during the mixing process of the inorganic filler and the amine-functionalized cellulose nanofibers, a high-speed stirrer is used to stir the mixture at a speed of 3000-3500 rpm for 0.8-1.2 hours to ensure uniform distribution of the filler.

[0023] Preferably, during the film casting process of step S3, a roller for adjusting the film thickness is used to control the thickness of the final product.

[0024] Preferably, in step S2, the preparation of the Nafion solution comprises dissolving the Nafion resin in a solvent containing ethanol and deionized water in a specific ratio to adjust the viscosity and rheology of the solution, wherein the ratio of ethanol to deionized water is 1:4 to 1:6.

[0025] Preferably, in step S4, after the oven heat treatment, a pressure treatment is further performed, wherein the pressure is 100 to 200 kPa, so as to enhance the structural stability of the membrane and reduce the generation of micropores.

[0026] Preferably, the proton exchange membrane is used as the electrolyte in the fuel cell.

[0027] The present invention provides a proton exchange membrane modified by doping with dual inorganic fillers. It has the following beneficial effects:

[0028] 1. The present invention significantly improves the hardness and compressive resistance of the composite membrane by anchoring CeO2 on amine-functionalized cellulose nanofibers (CNF) and adding SiO2 and Al2O3 nanoparticles. This structural reinforcement not only makes the membrane physically stronger, but also effectively resists the mechanical stress and wear that may occur during the operation of the fuel cell, thereby improving its service life and reliability.

[0029] 2. The addition of carbon nanotubes (CNT) of the present invention greatly enhances the electrical conductivity of the composite film. CNT, due to its unique one-dimensional structure and excellent electron conduction ability, can form an effective conductive network and promote the rapid transmission of protons. This is crucial to improving the output efficiency and response speed of fuel cells, and directly affects the overall energy conversion efficiency of the battery.

[0030] 3. The precise temperature control during the heat treatment process of the present invention and the subsequent baking step significantly improve the thermal stability of the composite film. By performing heat curing at a controlled temperature, not only the microstructure of the film is optimized, but also its performance stability under high temperature operating conditions is enhanced. Such treatment reduces the performance degradation problem caused by temperature fluctuations during long-term use.

[0031] 4. The introduction of CeO2 in the present invention brings excellent chemical stability to the composite membrane. These materials have strong antioxidant and chemical corrosion resistance characteristics, and can effectively protect the membrane from strong oxidants and corrosive chemicals in the operation of fuel cells. Improving chemical stability is the key to ensuring that the membrane maintains performance consistency in various chemical environments.

[0032] 5. In the present invention, the uniform distribution of inorganic fillers on CNF is ensured by precise solvent ratio and stirring conditions. Uniform distribution is the prerequisite for achieving uniform overall performance of the membrane and directly affects the quality and performance of the prepared membrane. In addition, this optimized solution ratio and stirring process also helps to reduce material waste and cost in the production process. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a diagram of a proton exchange membrane modified by doping with dual inorganic fillers. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings of the present invention specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example:

[0036] Please refer to the attached Figure 1 :

[0037] Example 1: Dual Inorganic Filler Doped Modified Proton Exchange Membrane Based on Standard Operating Conditions

[0038] step:

[0039] CeO2, SiO2 and Al2O3 nanoparticles were mixed with amine-functionalized cellulose nanofibers in the proportions of 2%, 1%, and 1%.

[0040] Stir at 3000 rpm for 1 hour to ensure uniform mixing.

[0041] The mixed amine-functionalized cellulose nanofibers were suspended in an ethanol and deionized water solution containing 15% Nafion.

[0042] The film casting process was carried out at 60°C, and the suspension was poured onto the film casting plate using a film casting machine, and the thickness was controlled at 100 μm.

[0043] After drying for 24 hours, the resulting product was heat treated at 80°C for 2 hours and compressed at a pressure of 100 kPa.

[0044] Summary: This example demonstrates a method for preparing a dual inorganic filler doped modified proton exchange membrane under standardized production conditions, which is suitable for large-scale production and ensures consistency and reliability of product quality.

[0045] Example 2: Enhanced proton exchange membrane for high temperature fuel cell

[0046] step:

[0047] The proportion of CeO2 was increased to 4% and mixed with amine-functionalized cellulose nanofibers.

[0048] Stirring was performed at 3500 rpm for 1.2 h to achieve better dispersion of the nanoparticles.

[0049] The suspension was prepared as in Example 1.

[0050] The film casting was performed at 70°C and the film thickness was adjusted to 150 μm to provide higher mechanical stability.

[0051] The heat treatment was carried out for a long time (3 hours) and post-treatment was carried out at a pressure of 200 kPa.

[0052] Summary: This embodiment is designed for a fuel cell operating in a high-temperature environment. The enhanced inorganic filler ratio and thickened membrane provide higher structural stability and long-term durability.

[0053] Example 3: Low-cost small-batch laboratory-scale sample preparation

[0054] step:

[0055] A lower proportion of inorganic fillers (1% each) was used for preliminary mixing.

[0056] The mixture was stirred at 2800 rpm for 0.8 h.

[0057] A lower concentration of Nafion solution (10%) was used for suspension preparation.

[0058] The film was cast at 100°C with a film thickness of 50 μm, suitable for laboratory testing.

[0059] The heat treatment was completed at 80 °C and 50 kPa pressure for 1 hour.

[0060] Summary: Suitable for the R&D stage or small-scale trials, this embodiment reduces material cost and preparation difficulty, and facilitates rapid iteration and testing of new formulations.

[0061] Example 4: Proton Exchange Membrane for Direct Methanol Fuel Cell

[0062] step:

[0063] The addition of carbon nanotubes (CNT) increased the ratio to 3% to enhance the conductivity.

[0064] The mixing and stirring steps are the same as in Example 1.

[0065] A high concentration of Nafion solution (20%) was used to enhance the ion exchange capacity of the membrane.

[0066] The casting temperature was maintained at 120°C and the film thickness was controlled at 120 μm.

[0067] Long-term heat treatment and high-pressure post-treatment to improve chemical stability and mechanical strength.

[0068] Summary: The exchange membrane designed for direct methanol fuel cells is adapted to higher chemical activity and operating requirements by increasing the CNT ratio and optimizing the Nafion content.

[0069] Example 5: Proton exchange membrane for outdoor applications with strong environmental adaptability

[0070] step:

[0071] The proportions of Al2O3 and SiO2 were increased to 2% each to improve environmental resistance.

[0072] The mixture was mixed under high speed stirring (3500 rpm) for 1.2 hours.

[0073] A diluted Nafion solution (12%) was used to prepare the suspension.

[0074] The films were cast at a relatively low temperature (60°C) to reduce thermal stress.

[0075] The structure was optimized by heat treatment at low temperature (60°C) for a long time and under low pressure (100 kPa).

[0076] Summary: It is suitable for use in outdoor environments with large temperature differences. This embodiment improves the environmental adaptability of the membrane by enhancing the material composition resistant to environmental corrosion and optimizing the low-temperature treatment process.

[0077] Summary:

[0078] These embodiments show the diverse applications of the proton exchange membrane of the present invention, from laboratory small-scale samples to solutions optimized for specific fuel cells, and each embodiment specifically adjusts the material ratio, preparation conditions and post-processing steps to adapt to different application requirements and environmental conditions. Through these embodiments, the proton exchange membrane of the present invention demonstrates its wide applicability and excellent performance in the field of fuel cells.

[0079] Comparative experiment:

[0080] The existing technical solution consists of:

[0081] The existing technology mainly uses unmodified NafionN membrane as the proton exchange membrane. NafionN is made of perfluorosulfonic acid polymer, which has good chemical stability and conductivity, but is susceptible to mechanical and chemical performance degradation under high temperature and extreme environment.

[0082] Experiment 1: Comparison of mechanical properties and pressure resistance

[0083] Purpose: To evaluate and compare the differences between the present invention and the prior art in terms of mechanical strength and compressive resistance.

[0084] method:

[0085] The unmodified NafionN membrane and the composite membrane proposed in the present invention were subjected to mechanical strength tests (such as tensile tests) and compression tests.

[0086] parameter:

[0087] Tensile Strength: Measures the maximum force (MPa) a film can withstand before breaking.

[0088] Elongation: The percentage elongation at the breaking point.

[0089] Compression strength: The degree of deformation (mm) and stress (MPa) in a compression test.

[0090] Experimental data:

[0091] Membrane Type Test Type Pressure / tension (MPa) Elongation / deformation degree (%) Pure Nafion Stretch 25 200 Pure Nafion compression 1 1.2 Film of the present invention Stretch 35 250 Film of the present invention compression 1.5 0.8

[0092] This experiment clearly shows that the composite membrane of the present invention is superior to pure Nafion membrane in terms of mechanical properties and pressure resistance. The hardness and pressure resistance of the composite membrane are significantly improved by the strategy of anchoring CeO2 and adding SiO2 and Al2O3 nanoparticles. The addition of these inorganic fillers effectively enhances the structural integrity of the membrane, making it more resistant to physical stress in long-term use and high-pressure environments. Experimental data show that the degree of deformation of the membrane of the present invention under the same pressure is significantly less than that of pure Nafion membrane, proving that its application in fuel cells will provide higher reliability and durability.

[0093] Experiment 2: Comparison of conductivity and temperature stability

[0094] Objective: To compare the conductivity of the composite membrane of the present invention and pure Nafion membrane as well as the conductivity changes at different temperatures.

[0095] method:

[0096] The resistivity of the different films was measured at room temperature, 50 °C and 80 °C using a four-point probe method.

[0097] parameter:

[0098] Conductivity: S / m, measured at different temperatures.

[0099] Experimental data:

[0100] Membrane Type Temperature(℃) Conductivity (S / m) Pure Nafion 25 0.1 Pure Nafion 80 0.14 Film of the present invention 25 0.15 Film of the present invention 80 0.25

[0101] The results of the comparative experiments on the conductivity performance show that the membrane of the present invention exhibits a higher conductivity than the pure Nafion membrane at both room temperature and high temperature conditions. The added carbon nanotubes (CNT) form an efficient conductive network in the membrane of the present invention, which significantly enhances the transmission efficiency of protons. In particular, in the high temperature test, the conductivity of the membrane of the present invention is significantly improved, indicating that it optimizes the microstructure and maintains better performance stability under high temperature operating conditions. This makes the membrane of the present invention particularly suitable for use in fuel cell systems that require high output efficiency and rapid response.

[0102] Experiment 3: Comparison of chemical stability and corrosion resistance

[0103] Objective: To evaluate the chemical stability of the composite membrane of the present invention and pure Nafion membrane in the presence of strong oxidants and corrosive chemicals.

[0104] method:

[0105] The two membranes were immersed in high concentration chloride solution and sulfuric acid solution respectively.

[0106] parameter:

[0107] Soaking time: 0, 24, 48, 72 hours.

[0108] Mass loss: %, indicates the mass change after chemical corrosion.

[0109] Surface Degradation: Use microscopy to evaluate changes in surface structure after chemical etching.

[0110] Experimental data:

[0111] Membrane Type Solution type Soaking time (one hour) Mass loss (%) Surface degradation score Pure Nafion chloride 72 2 Moderate Pure Nafion sulfuric acid 72 1.8 Moderate Film of the present invention chloride 72 0.8 slight Film of the present invention sulfuric acid 72 0.5 weak

[0112] In the environment of strong oxidants and corrosive chemicals, the composite membrane of the present invention exhibits excellent chemical stability and corrosion resistance. In the experiment, the mass loss and surface degradation of the membrane of the present invention when immersed in high-concentration chloride and sulfuric acid solutions were much lower than those of pure Nafion membranes. This is due to the introduction of CeO2, which not only enhances the oxidation resistance of the membrane, but also improves its ability to resist chemical corrosion. These results show that the membrane of the present invention can maintain its performance in more harsh chemical environments and is suitable for various chemically sensitive application scenarios.

[0113] Summary

[0114] Through the above three comparative experiments, we can clearly see that the dual inorganic filler doped modified proton exchange membrane provided by the present invention has significant improvements in mechanical properties, electrical conductivity, and chemical stability compared with the prior art. These improvements make the membrane of the present invention more suitable for wide application in modern fuel cell technology, especially in application scenarios requiring high performance and extreme environmental adaptability, providing a more reliable and efficient solution.

[0115] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A proton exchange membrane modified by doping with dual inorganic fillers, characterized in that: Contains the following ingredients: Nafion composite membrane matrix; CeO2 anchored on amine-functionalized cellulose nanofibers, wherein CeO2 accounts for 2% to 5% of the total mass of the composite membrane; Adding SiO2 nanoparticles, wherein the SiO2 nanoparticles account for 0.5% to 2% of the total weight of the composite film; Al2O3 nanoparticles are added, wherein the Al2O3 nanoparticles account for 0.5% to 2% of the total mass of the composite film.

2. A double inorganic filler doped and modified proton exchange membrane according to claim 1, characterized in that: The amine-functionalized cellulose nanofibers account for 3% to 7% of the total mass of the Nafion composite membrane matrix.

3. The double inorganic filler doped and modified proton exchange membrane according to claim 1, characterized in that: The particle sizes of CeO2, SiO2 and Al2O3 are all between 5 and 20 nanometers.

4. The double inorganic filler doped and modified proton exchange membrane according to claim 1, characterized in that: The method further comprises adding carbon nanotubes in an amount of 0.3% to 3% to enhance the mechanical properties and electrical conductivity of the composite film.

5. The method for preparing a proton exchange membrane doped and modified with dual inorganic fillers according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, mixing CeO2, SiO2 and Al2O3 nanoparticles with amine-functionalized cellulose nanofibers in a predetermined ratio to anchor these inorganic fillers on the surface of the amine-functionalized cellulose nanofibers; S2, suspending the treated amine-functionalized cellulose nanofibers in Nafion solution at room temperature to form a uniform suspension; S3, pouring the suspension into a flat film casting machine, and casting the film under the condition of controlling the temperature at 60° C. to 150° C.; S4. The cast membrane was dried at room temperature for 24 hours and then heat treated in an oven at 80° C. for 2 hours to complete the curing and performance optimization of the membrane.

6. The method for preparing a proton exchange membrane modified by doping with dual inorganic fillers according to claim 5, characterized in that: During the mixing of the inorganic filler and the amine-functionalized cellulose nanofibers, a high-speed stirrer is used to stir the mixture at a speed of 3000-3500 rpm for 0.8-1.2 hours to ensure uniform distribution of the filler.

7. The method for preparing a proton exchange membrane modified by doping with dual inorganic fillers according to claim 5, characterized in that: During the film casting process of step S3, a roller for adjusting the film thickness is used to control the thickness of the final product.

8. The method for preparing a proton exchange membrane doped and modified with dual inorganic fillers according to claim 5, characterized in that: In the step S2, the preparation of the Nafion solution includes dissolving the Nafion resin in a solvent containing ethanol and deionized water in a specific ratio to adjust the viscosity and rheology of the solution, wherein the ratio of ethanol to deionized water is 1:4 to 1:

6.

9. The method for preparing a proton exchange membrane doped and modified with dual inorganic fillers according to claim 5, characterized in that: In the step S4, after the oven heat treatment, a pressure treatment is further performed, wherein the pressure is 100 to 200 kPa, so as to enhance the structural stability of the membrane and reduce the generation of micropores.

10. A proton exchange membrane according to any one of claims 1 to 9 used as an electrolyte in a fuel cell.

Citation Information

Patent Citations

  • Organic-inorganic hybrid proton exchange membrane and preparation method and application thereof

    CN105576267A

  • Component modulation method of perfluorosulfonic acid resin membrane preparation liquid and prepared proton exchange membrane

    CN110148769A

  • Proton exchange membrane and preparation method and application thereof

    CN114665134A

  • Ion exchange membrane, method of making the ion exchange membrane, and flow battery comprising the ion exchange membrane

    TW202040860A

  • Electrolyte compositions for redox flow batteries

    US20220200030A1