Preparation method of aqueous flow battery based on metal ion-sugar complex
By using vanadium ion-glucosamine complex as electrolytes, the problem of low solubility of electrolytes in aqueous liquid flow batteries is solved, high energy density and long-term stability are achieved, and it is suitable for large-scale energy storage systems.
Patent Information
- Application Number
- CN202411170651.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-22
AI Technical Summary
The electrolyte solubility of aqueous liquid flow batteries is low, which limits the energy density and energy storage capacity of the battery, affecting its performance and stability.
The vanadium ion-glucosamine complex is used as the electrolyte and prepared by solvothermal method under an inert atmosphere to form an electrolyte with high solubility, high volume specific capacity and good cycle stability, thereby improving the ion concentration and conductivity of the battery.
It improves the energy density and energy storage capacity of the battery, ensures long-term and stable operation, is environmentally friendly and adjustable, and is suitable for large-scale energy storage systems.
Smart Images

Figure CN119009046A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemical energy storage, and in particular relates to a method for preparing an aqueous liquid flow battery based on a metal ion-sugar complex. Background Art
[0002] Energy storage technology plays a vital role in the transformation of renewable energy and power systems. With the rapid growth of renewable energy (such as solar and wind power), the demand for energy storage solutions is becoming increasingly urgent. Aqueous flow batteries, as one of the most popular energy storage technologies, store and release energy through the redox reaction of ions in the electrolyte.
[0003] Compared with traditional lithium-ion batteries, aqueous flow batteries have several advantages: they use widely available and renewable water and electrolytes as their main components, which enhances the sustainability of the battery; they have adjustable capacity and can meet energy storage needs of different scales by adjusting the capacity of the electrolyte and storage tank; they also have high energy conversion efficiency and long life, making them suitable for long-term energy storage and frequent charging and discharging applications.
[0004] However, aqueous flow batteries still face some challenges and problems in the field of energy storage. Among them, solubility is a key issue. The solubility of the electrolyte directly affects the performance of the aqueous flow battery. Lower solubility limits the concentration of the electrolyte, thereby reducing the energy density and energy storage capacity of the battery. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing an aqueous liquid flow battery based on a metal ion-sugar complex molecular system. The use of metal ion-sugar complexes as electrolytes for aqueous liquid flow batteries has the advantages of high solubility, high volumetric capacity, good cycle stability, adjustability and customizability, and environmental friendliness.
[0006] The technical solution adopted by the present invention is as follows:
[0007] On one hand, the present invention discloses a method for preparing an aqueous liquid flow battery based on a metal ion-sugar complex molecular system, and uses a vanadium ion-glucosamine complex as an electrolyte to prepare the aqueous liquid flow battery.
[0008] Furthermore, the vanadium ion-glucosamine complex is prepared by a solvothermal method under an inert atmosphere.
[0009] Furthermore, the preparation method of the vanadium ion-glucosamine complex comprises the following steps:
[0010] Step 1: Disperse glucosamine in a methanol solution, then add sodium methoxide and stir to form a light yellow emulsion;
[0011] Step 2: dissolving vanadium chloride in a methanol solution, and adding the solution in step 1 dropwise to form a brown precipitate; after stirring, collecting the precipitate by suction filtration, and washing it multiple times to obtain a mixture;
[0012] Step 3: vacuum drying the above mixture to obtain a vanadium ion-glucosamine complex.
[0013] Furthermore, in step 1, the usage ratio of glucosamine and methanol is (2-8) g: 100 mL;
[0014] The mass ratio of glucosamine and sodium methoxide is (0.83-1.66):1.
[0015] Further, in step 2, the usage ratio of vanadium chloride and methanol is (0.5-2) g: 50 mL;
[0016] The mass ratio of vanadium chloride to glucosamine is (0.22-0.44):1.
[0017] Furthermore, the stirring time in step 1 is 2 hours; and the stirring time in step 2 is 24 hours.
[0018] Furthermore, in step 2, methanol, acetonitrile and n-hexane are used for washing.
[0019] Furthermore, the vacuum drying in step 3 is carried out at 60°C.
[0020] Furthermore, a 1 M KCl aqueous solution was used as a supporting electrolyte.
[0021] Another aspect of the present invention discloses an aqueous liquid flow battery prepared by the preparation method of the present invention.
[0022] Beneficial effects of the present invention:
[0023] The preparation method of the aqueous liquid flow battery based on the metal ion-sugar complex molecular system and the aqueous liquid flow battery of the present invention propose a vanadium ion-glucosamine complex, which has the advantages of high solubility, high volumetric capacity, good cycle stability, adjustability and customizability, and environmental friendliness when used as the electrolyte of the aqueous liquid flow battery; its high solubility can increase the ion concentration and conductivity; the high volumetric capacity enables it to store more charge; good cycle stability ensures long-term stable operation; adjustability and customizability enable it to adapt to the needs of different battery systems; environmental friendliness makes it more sustainable and environmentally friendly; these advantages make the metal sugar complex a candidate material with potential for application in large-scale energy storage systems and liquid flow battery technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings are used to provide further explanation of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0025] Figure 1 is a spectral characterization diagram of V-Glu in Example 1 of the present invention;
[0026] Figure 2 are the test results of tests 1-3 in Example 2 of the present invention;
[0027] Figure 3 is the test result of Test 4 in Example 2 of the present invention;
[0028] Figure 4 This is the test result of the energy storage performance of the aqueous liquid flow battery in Example 3 of the present invention. DETAILED DESCRIPTION
[0029] In order to make the purpose and advantages of the present invention more clearly understood, the present invention is specifically described below in conjunction with embodiments. It should be understood that the following text is only used to describe one or several specific embodiments of the present invention, and does not strictly limit the scope of protection of the specific claims of the present invention.
[0030] Example 1
[0031] An aqueous liquid flow battery based on a metal ion-sugar complex molecular system, comprising an electrolyte, a positive electrode, a negative electrode, an electrolytic cell and a diaphragm. The structure and principle of this part are mature existing technologies and will not be described in detail in this technical solution.
[0032] The core of this technical solution is to use metal ion-sugar complex as electrolyte. Metal ion-sugar complex is composed of metal ions and sugar molecules, has high solubility, can increase the amount of ions dissolved in the battery, improve the ion concentration and conductivity of the battery; has good ionic conductivity, can provide faster ion transfer rate, enhance the power output and charge and discharge rate of the battery; has high chemical stability, can inhibit water decomposition reaction, improve the stability and cycle life of the battery; has design flexibility, and can meet specific application requirements through reasonable design and synthesis of regulatory structure.
[0033] A method for preparing an aqueous liquid flow battery based on a metal ion-sugar complex molecular system, wherein a vanadium ion-glucosamine complex is used as an electrolyte to prepare the aqueous liquid flow battery.
[0034] Among them, the metal ion-sugar complex is preferably a vanadium ion-glucosamine complex (V-Glu). The capacity of 1M vanadium ion-glucosamine complex after 100 cycles is 19.2Ah L -1 , the capacity retention rate reaches 95.5%;
[0035] At 60mA cm -2 At a current density of 1.5 Å, the capacity of the 0.2 M vanadium ion-glucosamine complex was 1.2 Ah L after 700 cycles. -1 , the capacity retention rate is 80%;
[0036] These results show that the vanadium ion-glucosamine complex has high solubility, high volumetric capacity and good cycle stability as the negative electrode side of the aqueous liquid flow battery. This structural design introduced based on the bionic concept has broad application prospects in the field of energy storage.
[0037] The vanadium ion-glucosamine complex is prepared by a solvothermal method under an inert atmosphere. In order to more clearly describe the vanadium ion-glucosamine complex, a preparation method of the vanadium ion-glucosamine complex is disclosed herein. The preparation method of the vanadium ion-glucosamine complex comprises the following steps:
[0038] Step 1: Disperse 5.39 g of glucosamine in 100 ml of methanol solution, then add 4.86 g of sodium methoxide, and stir the solution for 2 hours to form a light yellow emulsion;
[0039] Step 2: Dissolve 1.57 g of vanadium chloride in 50 ml of methanol solution, and add the solution dropwise to form a brown precipitate; after stirring for 24 hours, collect the precipitate by suction filtration, and wash it several times with methanol, acetonitrile, n-hexane and other solvents to obtain a mixture;
[0040] Step 3: The above mixture is vacuum dried at 60° C. to obtain the final product, vanadium ion-glucosamine complex (V-Glu).
[0041] The experiment used a solvothermal method and was carried out under an inert atmosphere to ensure the purity and stability of the preparation process. By gradually adding vanadium chloride solution, vanadium chloride can react with glucosamine to form a vanadium ion-glucosamine complex. After washing and drying steps, a pure vanadium ion-glucosamine complex product was finally obtained.
[0042] Figure 1 a- Figure 1 As shown in f, Figure 1 a is the infrared spectrum, Figure 1 b is the Raman spectrum, Figure 1 cf is the X-ray photoelectron spectrum, through Figure 1 a- Figure 1 The structural characterization in f can prove that trivalent vanadium is successfully coordinated with glucosamine.
[0043] In the technical solution, the electrolyte solution adopts 1M KCl aqueous solution as the supporting electrolyte, the electrolyte solution of the low-concentration battery system is 0.2M, and the electrolyte concentration of the high-concentration battery system is 1M.
[0044] Embodiment 2:
[0045] like Figure 2 a- Figure 3 As shown in Figure d, in order to verify the physical and chemical properties of the electrolyte, this embodiment performs the following tests on the electrolyte based on Example 1:
[0046] Test 1. Redox performance test: The redox properties of the electrolyte were analyzed by cyclic voltammetry using a standard three-electrode apparatus, in which a 50 mm diameter glassy carbon electrode was used as the working electrode, a platinum wire electrode was used as the counter electrode, and a saturated Ag / AgCl electrode was used as the reference electrode.
[0047] Test 2, transmembrane permeation test of electrolyte: The static diffusion method is used to test the transmembrane permeation degree of electrolyte; the test device is divided into two equal volume chambers (raw material side and receiving side), separated by an anion exchange membrane, and the solutions in the two chambers are continuously stirred during the test to make the concentration of the solution inside each chamber the same; the raw material side solution is 0.5M electrolyte dissolved in 1M KCl aqueous solution, and the receiving side is the same volume of 1M KCl aqueous solution; after one month, the concentration of the electrolyte in the receiving side solution is tested, and the characteristic peak intensity is tested using a UV-visible spectrophotometer.
[0048] Test 3, solubility test of vanadium ion-glucosamine complex: at room temperature, the vanadium ion-glucosamine complex was dissolved in water, stirred and ultrasonically treated, and electrolyte was continuously added to the solution until a precipitate was formed in the solution to obtain a saturated solution of electrolyte; the saturated solution was diluted a certain multiple, and the concentration of electrolyte in the diluted solution was measured by ultraviolet spectrophotometer, and then the solubility of the corresponding vanadium ion-glucosamine complex in water was calculated based on the dilution multiple.
[0049] Test 4: Diffusion coefficient test: Cyclic voltammetry tests were performed on the electrolyte at different scan rates using a standard three-electrode apparatus, and the diffusion coefficient was calculated using the Randles-Sevcik equation.
[0050] See also Figure 2 a- Figure 2 As shown in d, Figure 2 a is the UV absorption spectrum of V-Glu at different concentrations; Figure 2 b is the concentration test calculation of V-Glu; Figure 2 c is the transmembrane permeation degree of electrolytes tested by the static diffusion method of VCl3 and V-Glu after one month; Figure 2d is a comparison picture of VCl3 and V-Glu transmembrane tests; through comparison, it can be found that the solubility of the coordinated vanadium ion-glucosamine complex reaches 8.3M, and it performs excellently in the permeation experiment.
[0051] See also Figure 3 a- Figure 3 As shown in d, Figure 3 a and Figure 3 c is the kinetic characteristics and diffusion coefficient calculation of VCl3, Figure 3 b and Figure 3 d is the kinetic characteristics and diffusion coefficient calculation of V-Glu. By comparison, it was found that coordination has no negative impact on the ion diffusion rate of vanadium.
[0052] Embodiment 3:
[0053] This example tests the energy storage performance of the aqueous liquid flow battery based on Example 1, as follows:
[0054] This example uses the LAND CT2001A battery test system and a standard flow battery module to test battery performance. 2 The anion exchange membrane separates the cathode and anolyte; the reaction area is based on the area of the graphite felt electrode (5 cm 2 ); the electrolyte was pumped through a peristaltic pump (BT100-2J) at a rate of 70 mL min -1 The flow rate circulates between the battery and the tank;
[0055] Test a. Battery constant current charge and discharge test: Use LAND CT2001A battery test system to test different batteries at 40 and 60 mA cm -2 Constant current charge and discharge test at current density.
[0056] Test b: Battery rate performance test: Use LAND CT2001A battery test system to test the battery at 20-60mAcm -2 Constant current charge and discharge rate test under current density.
[0057] Test c: Battery constant current charge and discharge stability test: Use LAND CT2001A battery test system to test different batteries at 40 and 60 mA cm -2 Constant current charge and discharge test at current density.
[0058] like Figure 4 a- Figure 4 As shown in f, Figure 4 a is the charge and discharge curve of V-Glu at different current densities, Figure 4 b is the rate performance comparison between VCl3 and V-Glu. Figure 4c is the open circuit voltage test of V-Glu under different charging states, Figure 4 d is the power density test of V-Glu under different charging states. Figure 4 e is the constant current cycle test of VCl3 and V-Glu at 1M, Figure 4 f is the constant current cycling test of V-Glu at 0.2M; the constant current cycling stability test found that the vanadium-sugar complex has excellent stability during the charge and discharge process.
[0059] In summary, the present invention proposes a vanadium ion-glucosamine complex, which has the advantages of high solubility, high volumetric capacity, good cycle stability, adjustability and customizability, and environmental friendliness when used as an electrolyte for aqueous liquid flow batteries; its high solubility can increase ion concentration and conductivity; high volumetric capacity enables it to store more charge; good cycle stability ensures long-term stable operation; adjustability and customizability enable it to adapt to different battery system requirements; environmental friendliness makes it more sustainable and environmentally friendly; these advantages make the metal sugar complex a candidate material with potential for application in large-scale energy storage systems and liquid flow battery technology.
[0060] The vanadium ion-glucosamine complex aqueous flow battery based on the above design has a 222.2Ah L -1 The theoretical volumetric capacity. Compared with the traditional all-vanadium mud battery, the volumetric capacity is increased by 22 times, and it can operate in a neutral system; in addition, the 1M vanadium ion-glucosamine complex flow battery can operate at 40mA cm -2 The capacity retention rate of the 0.2M vanadium ion-glucosamine complex flow battery was 95.5% after 100 cycles at a current density of 60 mA cm -2 The capacity retention rate was 80% after 700 cycles at a current density of 1.58kWh; similar designs can be further extended to other traditional redox flow battery systems, bringing new vitality to environmentally friendly, high-capacity, large-scale energy storage.
[0061] The above is only a preferred embodiment of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principles of the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention shall be implemented according to the conventional means in the art unless otherwise specified and limited.
Claims
1. A method for preparing an aqueous liquid flow battery based on a metal ion-sugar complex molecular system, characterized in that: Aqueous flow batteries were prepared using vanadium ion-glucosamine complex as electrolyte.
2. The method for preparing an aqueous liquid flow battery based on a metal ion-sugar complex molecular system according to claim 1, characterized in that: The vanadium ion-glucosamine complex is prepared by a solvent thermal method under an inert atmosphere.
3. The method for preparing an aqueous flow battery based on a metal ion-sugar complex molecular system according to claim 1, characterized in that: The preparation method of the vanadium ion-glucosamine complex comprises the following steps: Step 1: Disperse glucosamine in a methanol solution, then add sodium methoxide and stir to form a light yellow emulsion; Step 2: dissolving vanadium chloride in a methanol solution, and adding the solution in step 1 dropwise to form a brown precipitate; after stirring, collecting the precipitate by suction filtration, and washing it multiple times to obtain a mixture; Step 3: vacuum drying the above mixture to obtain a vanadium ion-glucosamine complex.
4. The method for preparing an aqueous liquid flow battery based on a metal ion-sugar complex molecular system according to claim 3, characterized in that: In step 1, the dosage ratio of glucosamine and methanol is (2-8) g: 100 mL; The mass ratio of glucosamine and sodium methoxide is (0.83-1.66):
1.
5. The method for preparing an aqueous liquid flow battery based on a metal ion-sugar complex molecular system according to claim 3, characterized in that: In step 2, the usage ratio of vanadium chloride and methanol is (0.5-2) g: 50 mL; The mass ratio of vanadium chloride to glucosamine is (0.22-0.44):
1.
6. The method for preparing an aqueous liquid flow battery based on a metal ion-sugar complex molecular system according to claim 3, characterized in that: The stirring time in step 1 is 2 hours; the stirring time in step 2 is 24 hours.
7. The method for preparing an aqueous liquid flow battery based on a metal ion-sugar complex molecular system according to claim 3, characterized in that: In the step 2, methanol, acetonitrile and n-hexane are used for washing.
8. The method for preparing an aqueous flow battery based on a metal ion-sugar complex molecular system according to claim 3, characterized in that: The vacuum drying in step 3 is performed at 60°C.
9. The method for preparing an aqueous liquid flow battery based on a metal ion-sugar complex molecular system according to claim 1, characterized in that: A 1 M KCl aqueous solution was used as the supporting electrolyte.
10. An aqueous liquid flow battery, characterized in that: An aqueous liquid flow battery prepared by the preparation method described in any one of claims 1 to 9.