Solvent-assisted rapid method for preparing Spiro-OMeTAD layer of calcium titanium ore solar cell

By controlling wet oxidation in a pure oxygen atmosphere and adding bistrifluoroacetoxyiodobenzene, the problems of long oxidation time and poor stability of the Spiro-OMeTAD layer are solved, and the photoelectric conversion efficiency and device performance of perovskite solar cells are improved.

CN119012883APending Publication Date: 2024-11-22BEIJING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411308319.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The oxidation process of the Spiro-OMeTAD layer in existing perovskite solar cells is long and is easily affected by environmental humidity, resulting in unstable device performance. The added Li-TFSI is hygroscopic, which may damage the Spiro-OMeTAD layer structure and reduce photoelectricity. Conversion efficiency.

Method used

Control moisture oxidation in pure oxygen atmosphere, add bistrifluoroacetoxyiodine (PIFA) to Spiro-OMeTAD/lithium salt solution to shorten the oxidation time, improve hole mobility, and avoid the damage of water to the Spiro-OMeTAD structure .

Benefits of technology

It effectively shortens the oxidation time, improves the conductivity of Spiro-OMeTAD, improves the photoelectric conversion efficiency of perovskite solar cells, maintains the stability of the Spiro-OMeTAD layer, and reduces the manufacturing process cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005049914070000051
    Figure BDA0005049914070000051
  • Figure BDA0005049914070000071
    Figure BDA0005049914070000071
  • Figure BDA0005049914070000091
    Figure BDA0005049914070000091
Patent Text Reader

Abstract

The invention relates to a method for rapidly oxidizing a Spiro-OMeTAD layer of a perovskite solar cell with assistance of a solvent, and belongs to the technical field of perovskite solar cells. An electron transport layer SnO2, a perovskite active layer and a hole transport layer are sequentially prepared on transparent ITO glass subjected to cleaning pretreatment in a spin coating mode, then the transparent ITO glass is placed in an oxygen atmosphere with the humidity being 0-30% to be subjected to humidity control oxidation for 2-20 h, an oxidized Spiro-OMeTAD thin film is obtained, a metal electrode is evaporated on the oxidized Spiro-OMeTAD thin film, and the perovskite solar cell is obtained. And bis (trifluoroacetoxy) iodobenzene is added into a Spiro-OMeTAD mixed solution of the hole transport layer. According to the method for rapidly preparing the Spiro-OMeTAD layer of the calcium titanium ore solar cell, the damage to the Spiro-OMeTAD structure caused by long-time water oxidation can be avoided by controlling the oxidation humidity, and the bis (trifluoroacetoxyiodobenzene) is added into the Spiro-OMeTAD / lithium salt solution, so that the oxidation time can be greatly shortened, and the hole mobility of the Spiro-OMeTAD can be effectively improved. The highest photoelectric conversion efficiency of the perovskite solar cell device prepared by the method can reach 20.50%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer of a perovskite solar cell, belonging to the technical field of perovskite solar cells. Background Art

[0002] Solar energy is the most abundant energy on earth, which is inexhaustible. Therefore, the research on solar photovoltaic power generation system is of great significance to alleviate energy and environmental problems and improve energy consumption structure.

[0003] Among them, organic / inorganic hybrid halide perovskite solar cells, as a new generation of photovoltaic devices, have been widely studied and developed due to their advantages such as low environmental impact, low cost, simple preparation process, and high conversion efficiency. The hole transport layer that contacts the perovskite layer to extract holes plays an important role in the performance and stability of solar cells. Various hole transport layers have been successfully used to enhance device performance. Among them, Spiro-OMeTAD is still the most popular hole transport layer material for high-efficiency devices.

[0004] Since the original Spiro-OMeTAD film has a low hole mobility, it is usually necessary to add lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and 4-tert-butylpyridine (TBP) and continue the oxidation process in ambient air for dozens of hours. The oxidation mechanism is: (i) Spiro-OMeTAD + O2 = Spiro-OMeTAD·O2; (ii) Spiro-OMeTAD·O2 + LiTFSI = Spiro-OMeTAD + TFSI - +Li x O y Among them, LiTFSI is used to promote Spiro ·+ The generation of free radicals, while TBP is used to accelerate the dissolution of LiTFSI and optimize the film morphology. However, this oxidation takes a long time and has strict requirements on the oxidation environment. Different oxidation environments (such as humidity) will lead to different oxidation times, resulting in poor repeatability of device performance. At present, the existing technology still shortens the oxidation time by adjusting the oxidation humidity and temperature, but this technology still has some problems. For example, the added Li-TFSI is hygroscopic, and long-term oxidation will also damage the Spiro-OMeTAD layer structure and even endanger the perovskite layer, thereby greatly reducing the photoelectric conversion efficiency of perovskite solar cells. In addition, the use of other dopants or the use of new hole transport layer materials are also effective methods, but this will increase the cost of the manufacturing process. Summary of the invention

[0005] In response to the current technical problem of low photoelectric conversion efficiency of perovskite solar cells, the present invention proposes a method for solvent-assisted rapid oxidation of the Spiro-OMeTAD layer of perovskite solar cells. The present invention controls humidity oxidation in a pure oxygen atmosphere to avoid the damage of the Spiro-OMeTAD structure to the water content of long-term oxidation; and adds bis(trifluoroacetoxyiodobenzene) (PIFA) to the Spiro-OMeTAD / lithium salt solution of the hole transport layer, which can greatly shorten the oxidation time and effectively improve the hole mobility of Spiro-OMeTAD, thereby improving the photoelectric conversion efficiency of the perovskite solar cell.

[0006] A method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer of a perovskite solar cell, comprising the following steps:

[0007] An electron transport layer SnO2, a perovskite active layer and a hole transport layer are prepared by spin coating in sequence on a cleaned and pretreated transparent ITO glass; then, the glass is placed in an oxygen atmosphere with a humidity of 0 to 30% and oxidized for 2 to 20 hours to obtain an oxidized Spiro-OMeTAD film of the hole transport layer; and then, metal is evaporated on the oxidized Spiro-OMeTAD film to obtain a perovskite solar cell; bis(trifluoroacetoxyiodobenzene) PIFA is added to the Spiro-OMeTAD mixed solution of the hole transport layer.

[0008] Preferably, the Spiro-OMeTAD mixed solution of the hole transport layer further contains lithium bis(trifluoromethylsulfonyl)imide, 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, and 4-tert-butylpyridine.

[0009] Preferably, the amount of bis(trifluoroacetoxyiodobenzene) PIFA added to the Spiro-OMeTAD mixed solution is 1-3 mg / mL.

[0010] Preferably, the thickness of the electron transport layer SnO2 is 80-100 nm, the thickness of the perovskite active layer is 500-700 nm, and the thickness of the hole transport layer is 110-130 nm.

[0011] Preferably, the perovskite active layer material is FAPbI3, FA 1-x Cs x PbI, MAPbI3 or FA 1- z Cs z PbI x Br y Cl 3-x-y ; Among them, x=0~3, y=0~3, z=0~3.

[0012] The beneficial effects of the present invention are:

[0013] (1) The present invention controls humidity oxidation in a pure oxygen atmosphere to avoid the intrusion of moisture in the environment and damage to the Spiro-OMeTAD structure, thereby effectively improving the hole mobility of Spiro-OMeTAD;

[0014] (1) The oxidation method of the present invention using bis(trifluoroacetoxy)iodobenzene (PIFA) to assist in the oxidation of Spiro-OMeTAD can promote the oxidation of Spiro-OMeTAD. + The formation of Spiro-OMeTAD effectively improves the conductivity of Spiro-OMeTAD and greatly shortens the oxidation time. It also has the advantages of simple preparation process and low cost.

[0015] (2) The perovskite solar cell device prepared by the oxidation method of the present invention can achieve an efficiency of 20.50%, which is at a relatively high efficiency level among blank devices without any modification. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 JV curve of the perovskite solar cell prepared in Example 1;

[0017] Figure 2 JV curve of the perovskite solar cell prepared in Example 2;

[0018] Figure 3 JV curve of the perovskite solar cell prepared in Example 3;

[0019] Figure 4 SEM images of the oxidized Spiro-OMeTAD films prepared in Examples 1 to 3;

[0020] Figure 5 UV-Vis curves of the oxidized Spiro-OMeTAD films prepared in Example 1 and the comparative example. DETAILED DESCRIPTION

[0021] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.

[0022] Summary of the Invention

[0023] A method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer of a perovskite solar cell, comprising the following steps:

[0024] The electron transport layer SnO2, the perovskite active layer and the hole transport layer are prepared by spin coating in sequence on the cleaned and pretreated transparent ITO glass; then, the hole transport layer is placed in an oxygen atmosphere with a humidity of 0 to 30% and oxidized for 2 to 20 hours to obtain an oxidized Spiro-OMeTAD film of the hole transport layer, and then a metal electrode is evaporated on the oxidized Spiro-OMeTAD film to obtain a perovskite solar cell; the Spiro-OMeTAD mixed solution of the hole transport layer is added with bis(trifluoroacetoxyiodobenzene) PIFA, and the specific steps are as follows:

[0025] (1) ITO conductive glass cleaning pretreatment: The ITO conductive glass is cleaned with detergent solution, deionized water, anhydrous ethanol, acetone and anhydrous ethanol ultrasonic cleaning in sequence; the residual solution and air dust on the surface of the ITO conductive glass are blown clean with a nitrogen air gun, and then placed in a UV ozone cleaning machine for 30 to 40 minutes to improve the wettability of the ITO conductive glass substrate;

[0026] (2) Preparation of SnO2 electron transport layer: Add SnO2 nano-aqueous solution to deionized water and mix well, seal and ultrasonicate for 5-10 min, filter impurities and prepare SnO2 precursor solution; drop the SnO2 precursor solution onto the ITO conductive glass substrate, spin coat at 4000-6000 r / min for 30-40 s, anneal at 150-180°C for 20-30 min, cool to room temperature, transfer to UV ozone cleaning machine and clean for 15-20 min to obtain a uniform and dense SnO2 electron transport layer;

[0027] (3) Preparation of perovskite light absorbing layer: Add dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) to a mixture of PbI2 and CsI in a glove box, mix well, and stir and dissolve at a temperature of 70 to 80°C to obtain an inorganic solution; the volume ratio of dimethylformamide (DMF) to dimethyl sulfoxide (DMSO) is 9:1; the concentration of PbI2 in the inorganic solution is 600 to 691.5 mg / mL, and the molar ratio of PbI2 to CsI is 12 to 14:1;

[0028] Adding isopropyl alcohol (IPA) solution to a mixture of formamidine iodide (FAI) and methylammonium chloride (MACl), stirring and dissolving to obtain an organic solution; the mass ratio of formamidine iodide (FAI) to methylammonium chloride (MACl) is 10:1, and the concentration of methylammonium chloride (MACl) in the organic solution is 7-9 mg / mL;

[0029] The inorganic solution is uniformly dropped on the SnO2 electron transport layer, and the solution is spin-coated at a speed of 2000-3000 r / min for 30-40 seconds, and then annealed at a temperature of 70-80°C for 60-80 seconds, and then cooled to room temperature to obtain an inorganic thin film layer; the organic solution is dropped on the center of the inorganic thin film layer, and the solution is spin-coated at a speed of 2400-3200 r / min for 30-40 seconds, and then annealed at a temperature of 150-180°C for 30-40 minutes to obtain a perovskite light absorption layer FACsPbI3 thin film;

[0030] (4) Preparation of hole transport layer: Lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) was dissolved in acetonitrile to prepare a lithium salt solution; 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) was dissolved in chlorobenzene solution, and then the lithium salt solution and 4-tert-butylpyridine (TBP) solution were added and stirred to dissolve to prepare a Spiro-OMeTAD / lithium salt solution; finally, the Spiro-OMeTAD was added. D / adding bis(trifluoroacetoxyiodobenzene) (PIFA) to the lithium salt solution to obtain a Spiro-OMeTAD mixed solution; in the Spiro-OMeTAD mixed solution, the concentration of Spiro-OMeTAD is 70-80 mg / mL, the concentration of LiTFSI is 7-9 mg / mL, the concentration of bis(trifluoroacetoxyiodobenzene) (PIFA) is 1-3 mg / mL, and the amount of 4-tert-butylpyridine (TBP) solution with a mass concentration of 98% is added in an amount of 20-30 μL / mL;

[0031] The Spiro-OMeTAD mixed solution was drop-coated on the center of the perovskite light-absorbing layer FACsPbI3 film, and spin-coated at a speed of 3000-4000 r / min for 30-40s to obtain a hole transport layer, which was then stored in a light-shielded environment.

[0032] (5) Oxidation of Spiro-OMeTAD in the hole transport layer: placing the solar cell with the hole transport layer in a vacuum tank, evacuating the vacuum, introducing oxygen, and performing humidity-controlled oxidation for 2 to 20 hours in an oxygen atmosphere with a humidity of 0 to 30% to obtain an oxidized Spiro-OMeTAD film;

[0033] (6) Metal evaporation: In a glove box, the electron transport layer SnO2, the perovskite layer FACsPbI3 and the hole transport layer are scraped off to expose the ITO conductive glass substrate, which is then placed in a evaporation chamber and evaporated to a preset thickness under vacuum conditions to obtain a perovskite solar cell.

[0034] Preferably, the thickness of the electron transport layer SnO2 is 80-100 nm, the thickness of the perovskite layer FACsPbI3 is 500-700 nm, and the thickness of the hole transport layer is 110-130 nm;

[0035] Preferably, the humidity of the oxygen atmosphere is 0-10%, and the oxidation is carried out for 14-20 hours;

[0036] Preferably, the humidity of the oxygen atmosphere is 10-20%, and the oxidation is performed for 8-14 hours;

[0037] Preferably, the humidity of the oxygen atmosphere is 20-30%, and the oxidation is performed for 2-8 hours;

[0038] The present invention controls humidity oxidation in a pure oxygen atmosphere to avoid damage to the structure of Spiro-OMeTAD by moisture in the environment, and adds bis(trifluoroacetoxy)iodobenzene (PIFA) to the Spiro-OMeTAD / lithium salt solution, which can effectively promote the oxidation of Spiro-OMeTAD. + The formation of ions improves the hole mobility of Spiro-OMeTAD and greatly shortens the oxidation time.

[0039] Example 1: A method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer of a perovskite solar cell, the specific steps are as follows:

[0040] (1) ITO conductive glass cleaning pretreatment: The ITO conductive glass was ultrasonically cleaned with detergent solution, deionized water, anhydrous ethanol, acetone and anhydrous ethanol for 25 minutes in sequence; the residual solution and air dust on the surface of the ITO conductive glass were blown clean with a nitrogen gun, and then placed in a UV ozone cleaning machine for 30 minutes to improve the wettability of the ITO conductive glass substrate;

[0041] (2) Preparation of SnO2 electron transport layer: A 15% SnO2 nano-aqueous solution was mixed evenly with deionized water in a volume ratio of 1:6, sealed and ultrasonically treated for 5 minutes, impurities were filtered out, and a SnO2 precursor solution was prepared; the SnO2 precursor solution was drop-coated on an ITO conductive glass substrate, spin-coated at a speed of 4000 r / min for 30 seconds, and then annealed at a temperature of 150°C for 30 minutes, cooled to room temperature, and transferred to a UV ozone cleaning machine for cleaning for 15 minutes to obtain a uniform and dense SnO2 electron transport layer; the thickness of the SnO2 electron transport layer was 100 nm;

[0042] (3) Preparation of perovskite light absorbing layer: In a glove box, dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) were added to a mixture of PbI2 and CsI, mixed evenly, and stirred and dissolved at 70°C to obtain an inorganic solution; the volume ratio of dimethylformamide (DMF) to dimethyl sulfoxide (DMSO) was 9:1; the concentration of PbI2 in the inorganic solution was 600 mg / mL, and the molar ratio of PbI2 to CsI was 12:1;

[0043] Adding isopropanol (IPA) solution to a mixture of formamidine iodide (FAI) and methylammonium chloride (MACl), stirring and dissolving to obtain an organic solution; the mass ratio of formamidine iodide (FAI) to methylammonium chloride (MACl) is 10:1, and the concentration of methylammonium chloride (MACl) in the organic solution is 7 mg / mL;

[0044] The inorganic solution is uniformly dropped on the SnO2 electron transport layer, and the layer is spin-coated at a speed of 2000 r / min for 30 seconds, and then annealed at a temperature of 70°C for 80 seconds, and then cooled to room temperature to obtain an inorganic thin film layer; the organic solution is dropped on the center of the inorganic thin film layer, and the layer is spin-coated at a speed of 2400 r / min for 40 seconds, and then annealed at a temperature of 150°C for 40 minutes to obtain a perovskite light absorption layer FACsPbI3 thin film; the perovskite layer FACsPbI3 has a thickness of 500 nm;

[0045] (4) Preparation of hole transport layer: dissolving lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) in acetonitrile solution to prepare a lithium salt solution; dissolving 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) in chlorobenzene solution, adding lithium salt solution and 4-tert-butylpyridine (TBP) solution and stirring to dissolve to prepare a Spiro-OMeTAD / lithium salt solution; finally, adding bis(trifluoroacetoxyiodobenzene) (PIFA) to the Spiro-OMeTAD / lithium salt solution to obtain a Spiro-OMeTAD mixed solution; in the Spiro-OMeTAD mixed solution, the concentration of Spiro-OMeTAD is 70 mg / mL, the concentration of LiTFSI is 7 mg / mL, the concentration of bis(trifluoroacetoxyiodobenzene) (PIFA) is 1 mg / mL, and the amount of 4-tert-butylpyridine (TBP) solution with a mass concentration of 98% is added in an amount of 20 μL / mL;

[0046] The Spiro-OMeTAD mixed solution was drop-coated on the center of the perovskite light-absorbing layer FACsPbI3 film, and the film was spin-coated at a speed of 3000 r / min for 40 seconds to obtain a hole transport layer, which was then shielded from light and stored; the thickness of the hole transport layer was 110 nm;

[0047] (5) Oxidation of Spiro-OMeTAD in the hole transport layer: The solar cell prepared with the hole transport layer is placed in a vacuum tank, evacuated, and oxygen is introduced to oxidize it in an oxygen atmosphere with a humidity of 0 to 10% for 14 to 20 hours to obtain an oxidized Spiro-OMeTAD film;

[0048] (6) Metal evaporation: In a glove box, the electron transport layer SnO2, the perovskite layer FACsPbI3 and the hole transport layer are scraped off to expose the ITO conductive glass substrate, which is then placed in a evaporation chamber and evaporated to a preset thickness (100 nm) of metal (such as Au) under vacuum conditions to obtain a perovskite solar cell;

[0049] The photoelectric conversion efficiency of the perovskite solar cell of this embodiment was tested on a solar simulator (see Table 1).

[0050] Table 1 Photovoltaic conversion efficiency of different perovskite solar cells

[0051]

[0052]

[0053] As shown in Table 1, in an oxygen atmosphere with an oxidation humidity of 0 to 10%, the time required for oxidation gradually decreases with the increase of the oxidation humidity, indicating that a certain humidity can promote the oxidation of Spiro-OMeTAD; the device efficiency is basically the same under an oxidation humidity of 0 to 6%, among which the JV curve prepared by controlled humidity oxidation for 17 hours in an oxygen atmosphere with a humidity of 5% is shown in Table 1. Figure 1 , open circuit voltage (Voc) is 1.08V, short circuit current density (Jsc) is 24.70mA / cm 2 , the fill factor (FF) is 77% and the device efficiency is 20.50%; when the oxidation humidity is further increased to 8-10%, the device efficiency will decrease by about 0.5%.

[0054] Example 2: A method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer of a perovskite solar cell, the specific steps are as follows:

[0055] (1) ITO conductive glass cleaning pretreatment: The ITO conductive glass was ultrasonically cleaned with detergent solution, deionized water, anhydrous ethanol, acetone and anhydrous ethanol for 30 minutes in sequence; the residual solution and air dust on the surface of the ITO conductive glass were blown clean with a nitrogen air gun, and then placed in a UV ozone cleaning machine for 35 minutes to improve the wettability of the ITO conductive glass substrate;

[0056] (2) Preparation of SnO2 electron transport layer: A 15% SnO2 nano-aqueous solution was mixed evenly with deionized water in a volume ratio of 1:6, sealed and ultrasonically treated for 8 minutes, impurities were filtered out, and a SnO2 precursor solution was prepared; the SnO2 precursor solution was drop-coated on an ITO conductive glass substrate, spin-coated at a speed of 5000 r / min for 40 seconds, and then annealed at a temperature of 160°C for 25 minutes, cooled to room temperature, and transferred to a UV ozone cleaning machine for cleaning for 18 minutes to obtain a uniform and dense SnO2 electron transport layer; the thickness of the SnO2 electron transport layer was 90 nm;

[0057] (3) Preparation of perovskite light absorbing layer: In a glove box, dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) were added to a mixture of PbI2 and CsI, mixed evenly, and stirred and dissolved at a temperature of 75°C to obtain an inorganic solution; the volume ratio of dimethylformamide (DMF) to dimethyl sulfoxide (DMSO) was 9:1; the concentration of PbI2 in the inorganic solution was 645.75 mg / mL, and the molar ratio of PbI2 to CsI was 13:1;

[0058] Adding isopropanol (IPA) solution to a mixture of formamidine iodide (FAI) and methylammonium chloride (MACl), stirring and dissolving to obtain an organic solution; the mass ratio of formamidine iodide (FAI) to methylammonium chloride (MACl) is 10:1, and the concentration of methylammonium chloride (MACl) in the organic solution is 8 mg / mL;

[0059] The inorganic solution was uniformly dropped on the SnO2 electron transport layer, and the layer was spin-coated at a speed of 2500 r / min for 35 seconds, and then annealed at a temperature of 75°C for 70 seconds, and then cooled to room temperature to obtain an inorganic thin film layer; the organic solution was dropped on the center of the inorganic thin film layer, and the layer was spin-coated at a speed of 2800 r / min for 35 seconds, and then annealed at a temperature of 160°C for 35 minutes to obtain a perovskite light absorption layer FACsPbI3 thin film; the perovskite layer FACsPbI3 had a thickness of 600 nm;

[0060] (4) Preparation of hole transport layer: dissolving lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) in acetonitrile solution to prepare a lithium salt solution; dissolving 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) in chlorobenzene solution, adding lithium salt solution and 4-tert-butylpyridine (TBP) solution and stirring to dissolve to prepare Spiro-OMeTAD / lithium salt solution; finally, adding bis(trifluoroacetoxyiodobenzene) (PIFA) to the Spiro-OMeTAD / lithium salt solution to obtain a Spiro-OMeTAD mixed solution; in the Spiro-OMeTAD mixed solution, the concentration of Spiro-OMeTAD is 75 mg / mL, the concentration of LiTFSI is 8 mg / mL, the concentration of bis(trifluoroacetoxyiodobenzene) (PIFA) is 2 mg / mL, and the amount of 4-tert-butylpyridine (TBP) solution with a mass concentration of 98% is added in an amount of 25 μL / mL;

[0061] The Spiro-OMeTAD mixed solution was drop-coated on the center of the perovskite light-absorbing layer FACsPbI3 film, and the film was spin-coated at a speed of 3500 r / min for 35 seconds to obtain a hole transport layer, which was then shielded from light and stored; the thickness of the hole transport layer was 120 nm;

[0062] (5) Oxidation of Spiro-OMeTAD in the hole transport layer: The solar cell prepared with the hole transport layer is placed in a vacuum tank, evacuated, and oxygen is introduced to oxidize it in an oxygen atmosphere with a humidity of 10 to 20% for 8 to 14 hours to obtain an oxidized Spiro-OMeTAD film;

[0063] (6) Metal evaporation: In a glove box, the electron transport layer SnO2, the perovskite layer FACsPbI3 and the hole transport layer are scraped off to expose the ITO conductive glass substrate, which is then placed in a evaporation chamber and evaporated to a preset thickness (100 nm) of metal (such as Au) under vacuum conditions to obtain a perovskite solar cell;

[0064] The photoelectric conversion efficiency of the perovskite solar cell of this embodiment was tested on a solar simulator (see Table 2).

[0065] Table 2 Photovoltaic conversion efficiency of different perovskite solar cells

[0066]

[0067] As shown in Table 2, in an oxidizing atmosphere with an oxidation humidity of 10-20%, the time required for the oxidation of Spiro-OMeTAD is further gradually reduced, and as the oxidation humidity increases, the open circuit voltage and fill factor decrease, resulting in a significant decrease in efficiency of about 2%, indicating that high humidity has a bad effect on the Spiro-OMeTAD layer; the JV curve prepared by controlled humidity oxidation for 11h in an oxygen atmosphere with a humidity of 15% is shown in FIG. Figure 2 , the circuit voltage (Voc) is 1.07V, and the short-circuit current density (Jsc) is 23.53mA / cm 2 , the fill factor (FF) is 74% and the device efficiency is 18.72%.

[0068] Example 3: A method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer of a perovskite solar cell, the specific steps are as follows:

[0069] (1) ITO conductive glass cleaning pretreatment: The ITO conductive glass was ultrasonically cleaned with detergent solution, deionized water, anhydrous ethanol, acetone and anhydrous ethanol for 35 minutes in sequence; the residual solution and air dust on the surface of the ITO conductive glass were blown clean with a nitrogen gun, and then placed in a UV ozone cleaning machine for 40 minutes to improve the wettability of the ITO conductive glass substrate;

[0070] (2) Preparation of SnO2 electron transport layer: A 15% SnO2 nano-aqueous solution was mixed evenly with deionized water in a volume ratio of 1:6, sealed and ultrasonically treated for 10 min, impurities were filtered out, and a SnO2 precursor solution was prepared; the SnO2 precursor solution was drop-coated on an ITO conductive glass substrate, spin-coated at a speed of 6000 r / min for 32 s, and then annealed at a temperature of 180°C for 20 min, cooled to room temperature, and transferred to a UV ozone cleaning machine for cleaning for 20 min to obtain a uniform and dense SnO2 electron transport layer; the thickness of the SnO2 electron transport layer was 100 nm;

[0071] (3) Preparation of perovskite light absorbing layer: In a glove box, dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) were added to a mixture of PbI2 and CsI, mixed evenly, and stirred and dissolved at a temperature of 80°C to obtain an inorganic solution; the volume ratio of dimethylformamide (DMF) to dimethyl sulfoxide (DMSO) was 9:1; the concentration of PbI2 in the inorganic solution was 691.5 mg / mL, and the molar ratio of PbI2 to CsI was 14:1;

[0072] Adding isopropyl alcohol (IPA) solution to a mixture of formamidine iodide (FAI) and methylammonium chloride (MACl), stirring and dissolving to obtain an organic solution; the mass ratio of formamidine iodide (FAI) to methylammonium chloride (MACl) is 10:1, and the concentration of methylammonium chloride (MACl) in the organic solution is 9 mg / mL;

[0073] The inorganic solution is uniformly dropped on the SnO2 electron transport layer, and the layer is spin-coated at a speed of 3000 r / min for 40 seconds, and then annealed at a temperature of 80°C for 60 seconds, and then cooled to room temperature to obtain an inorganic thin film layer; the organic solution is dropped on the center of the inorganic thin film layer, and the layer is spin-coated at a speed of 3200 r / min for 30 seconds, and then annealed at a temperature of 180°C for 30 minutes to obtain a perovskite light absorption layer FACsPbI3 thin film; the perovskite layer FACsPbI3 has a thickness of 700 nm;

[0074] (4) Preparation of hole transport layer: dissolving lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) in acetonitrile solution to prepare a lithium salt solution; dissolving 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) in chlorobenzene solution, adding lithium salt solution and 4-tert-butylpyridine (TBP) solution and stirring to dissolve to prepare Spiro-OMeTAD / lithium salt solution; finally, adding bis(trifluoroacetoxyiodobenzene) (PIFA) to the Spiro-OMeTAD / lithium salt solution to obtain a Spiro-OMeTAD mixed solution; in the Spiro-OMeTAD mixed solution, the concentration of Spiro-OMeTAD is 80 mg / mL, the concentration of LiTFSI is 9 mg / mL, the concentration of bis(trifluoroacetoxyiodobenzene) (PIFA) is 3 mg / mL, and 30 μL / mL of 4-tert-butylpyridine (TBP) solution with a mass concentration of 98% is added;

[0075] The Spiro-OMeTAD mixed solution was drop-coated on the center of the perovskite light-absorbing layer FACsPbI3 film, and the film was spin-coated at a speed of 4000 r / min for 30 seconds to obtain a hole transport layer, which was then shielded from light and stored; the thickness of the hole transport layer was 130 nm;

[0076] (5) Oxidation of Spiro-OMeTAD in the hole transport layer: The solar cell prepared with the hole transport layer is placed in a vacuum tank, evacuated, and oxygen is introduced to oxidize it in an oxygen atmosphere with a humidity of 20 to 30% for 2 to 8 hours to obtain an oxidized Spiro-OMeTAD film;

[0077] (6) Metal evaporation: In a glove box, the electron transport layer SnO2, the perovskite layer FACsPbI3 and the hole transport layer are scraped off to expose the ITO conductive glass substrate, which is then placed in a evaporation chamber and evaporated to a preset thickness (100 nm) of metal (such as Au) under vacuum conditions to obtain a perovskite solar cell;

[0078] The photoelectric conversion efficiency of the perovskite solar cell of this embodiment was tested on a solar simulator (see Table 3).

[0079] Table 3 Photovoltaic conversion efficiency of different perovskite solar cells

[0080]

[0081] As can be seen from Table 3, in an oxidation atmosphere with an oxidation humidity of 20-30%, the time required for the oxidation of Spiro-OMeTAD is further gradually reduced, and with the increase of the oxidation humidity, the open circuit voltage and the fill factor further decrease, resulting in a greater decrease in efficiency, about 3%, indicating that the Spiro-OMeTAD layer has been severely damaged; in order to compare our oxidation environment, we carried out oxidation in an air atmosphere and found that its efficiency has dropped significantly, indicating that the humidity in the air is greater and the damage to the Spiro-OMeTAD layer is more serious; the JV curve prepared by controlled humidity oxidation for 5 hours in an oxygen atmosphere with a humidity of 25% is shown in FIG. Figure 3 , the circuit voltage (Voc) is 1.02V, and the short circuit current density (Jsc) is 23.03mA / cm 2 , the fill factor (FF) is 70% and the device efficiency is 16.52%;

[0082] In Example 1, the oxidized Spiro-OMeTAD film was obtained by controlled wet oxidation in an oxygen atmosphere with a humidity of 5% for 17 hours, in Example 2, the oxidized Spiro-OMeTAD film was obtained by controlled wet oxidation in an oxygen atmosphere with a humidity of 15% for 11 hours, and in Example 3, the oxidized Spiro-OMeTAD film was obtained by controlled wet oxidation in an oxygen atmosphere with a humidity of 25% for 5 hours. The SEM images are shown in FIG. Figure 4 ,from Figure 4It can be seen that when the oxidation humidity is about 5%, the Spiro-OMeTAD film is very dense, but there are also a small number of pinholes; when the humidity increases to about 15%, a large number of bulges appear on the surface of the Spiro-OMeTAD film, indicating that water molecules enter from the pinholes and react with the Spiro-OMeTAD layer to produce gaseous substances; when the humidity further increases to about 25%, due to the production of more gaseous substances, its pressure exceeds the adhesion between the perovskite layer and the Spiro-OMeTAD layer, so the bulges rupture, resulting in more defects in the Spiro-OMeTAD layer; as the humidity gradually increases, the Spiro-OMeTAD layer is gradually damaged, which is consistent with the gradual deterioration of device performance, indicating that moisture is not conducive to the oxidation of Spiro-OMeTAD.

[0083] Comparative Example: A method for oxidizing a Spiro-OMeTAD layer of a perovskite solar cell, the specific steps are as follows:

[0084] (1) ITO conductive glass cleaning pretreatment: The ITO conductive glass was ultrasonically cleaned with detergent solution, deionized water, anhydrous ethanol, acetone and anhydrous ethanol for 25 minutes in sequence; the residual solution and air dust on the surface of the ITO conductive glass were blown clean with a nitrogen gun, and then placed in a UV ozone cleaning machine for 30 minutes to improve the wettability of the ITO conductive glass substrate;

[0085] (2) Preparation of SnO2 electron transport layer: A 15% SnO2 nano-aqueous solution was mixed evenly with deionized water in a volume ratio of 1:6, sealed and ultrasonically treated for 5 minutes, impurities were filtered out, and a SnO2 precursor solution was prepared; the SnO2 precursor solution was drop-coated on an ITO conductive glass substrate, spin-coated at a speed of 4000 r / min for 30 seconds, and then annealed at a temperature of 150°C for 30 minutes, cooled to room temperature, and transferred to a UV ozone cleaning machine for cleaning for 15 minutes to obtain a uniform and dense SnO2 electron transport layer; the thickness of the SnO2 electron transport layer was 100 nm;

[0086] (3) Preparation of perovskite light absorbing layer: In a glove box, dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) were added to a mixture of PbI2 and CsI, mixed evenly, and stirred and dissolved at 70°C to obtain an inorganic solution; the volume ratio of dimethylformamide (DMF) to dimethyl sulfoxide (DMSO) was 9:1; the concentration of PbI2 in the inorganic solution was 600 mg / mL, and the molar ratio of PbI2 to CsI was 12:1;

[0087] Adding isopropanol (IPA) solution to a mixture of formamidine iodide (FAI) and methylammonium chloride (MACl), stirring and dissolving to obtain an organic solution; the mass ratio of formamidine iodide (FAI) to methylammonium chloride (MACl) is 10:1, and the concentration of methylammonium chloride (MACl) in the organic solution is 7 mg / mL;

[0088] The inorganic solution is uniformly dropped on the SnO2 electron transport layer, and the layer is spin-coated at a speed of 2000 r / min for 30 seconds, and then annealed at a temperature of 70°C for 80 seconds, and then cooled to room temperature to obtain an inorganic thin film layer; the organic solution is dropped on the center of the inorganic thin film layer, and the layer is spin-coated at a speed of 2400 r / min for 40 seconds, and then annealed at a temperature of 150°C for 40 minutes to obtain a perovskite light absorption layer FACsPbI3 thin film; the perovskite layer FACsPbI3 has a thickness of 500 nm;

[0089] (4) Preparation of hole transport layer: dissolve lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) in acetonitrile solution to prepare a lithium salt solution; dissolve 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD) in chlorobenzene solution, add lithium salt solution and 4-tert-butylpyridine (TBP) solution and stir to dissolve to prepare Spiro-OMeTAD / lithium salt solution; the Spiro-OMeTAD concentration in the Spiro-OMeTAD / lithium salt solution is 70 mg / mL, the LiTFSI concentration is 7 mg / mL, and 20 μL of 4-tert-butylpyridine (TBP) solution with a mass concentration of 98% is added;

[0090] The Spiro-OMeTAD / lithium salt solution was drop-coated on the center of the perovskite light-absorbing layer FACsPbI3 film, and the film was spin-coated at a speed of 3000 r / min for 40 seconds to obtain a hole transport layer, which was then shielded from light and stored; the thickness of the hole transport layer was 110 nm;

[0091] (5) Oxidation of Spiro-OMeTAD in the hole transport layer: The solar cell prepared with the hole transport layer is placed in a vacuum tank, evacuated, and oxygen is introduced to oxidize it in an oxygen atmosphere with a humidity of 0 to 10% for 62 to 72 hours to obtain an oxidized Spiro-OMeTAD film;

[0092] (6) Metal evaporation: In a glove box, the electron transport layer SnO2, the perovskite layer FACsPbI3 and the hole transport layer are scraped off to expose the ITO conductive glass substrate, which is then placed in a evaporation chamber. Under vacuum conditions, metal (such as Au) is evaporated to a preset thickness (100 nm) to obtain a perovskite solar cell. The photoelectric conversion efficiency of the perovskite solar cell of this comparative example is tested in a solar simulator (see Table 4).

[0093] Table 4 Photovoltaic conversion efficiency of different perovskite solar cells

[0094]

[0095] As shown in Table 4, when PIFA is not added, the efficiency of the battery is not reduced when Spiro-OMeTAD is oxidized at a humidity of 0 to 10%, but the oxidation time of Spiro-OMeTAD increases by 3 to 4 times, indicating that the addition of PIFA can promote the oxidation process and greatly reduce the oxidation time. Figure 5 As shown in the UV-Vis spectra, the Spiro-OMeTAD film with bis(trifluoroacetoxyiodobenzene) (PIFA) added exhibits a clear absorption peak at about 520 nm, which is the result of the oxidation of Spiro-OMeTAD. + The color of the Spiro-OMeTAD solution also changes from light yellow to purple-red; therefore, PIFA has a strong oxidizing ability and undergoes oxidation reaction in the Spiro-OMeTAD solution, resulting in the rapid and efficient production of a large amount of Spiro-OMeTAD + Free radicals.

[0096] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer in a perovskite solar cell, characterized in that: The specific steps are as follows: An electron transport layer SnO2, a perovskite active layer and a hole transport layer are prepared by spin coating in sequence on a cleaned and pretreated transparent ITO glass; then, the glass is placed in an oxygen atmosphere with a humidity of 0 to 30% and oxidized for 2 to 20 hours to obtain an oxidized Spiro-OMeTAD film of the hole transport layer; a metal electrode is then evaporated on the oxidized Spiro-OMeTAD film to obtain a perovskite solar cell; bis(trifluoroacetoxyiodobenzene) PIFA is added to the Spiro-OMeTAD mixed solution of the hole transport layer.

2. The method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer in a perovskite solar cell according to claim 1, characterized in that: The humidity of the oxygen atmosphere is 0-10%, and the oxidation is carried out for 14-20 hours.

3. The method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer in a perovskite solar cell according to claim 1, characterized in that: The humidity of the oxygen atmosphere is 10-20%, and the oxidation time is 8-14 hours.

4. The method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer in a perovskite solar cell according to claim 1, characterized in that: The humidity of the oxygen atmosphere is 20-30%, and the oxidation time is 2-8 hours.

5. The method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer in a perovskite solar cell according to claim 1, characterized in that: The Spiro-OMeTAD mixed solution of the hole transport layer also contains lithium bis(trifluoromethylsulfonyl)imide, 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, and 4-tert-butylpyridine.

6. The method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer in a perovskite solar cell according to claim 5, characterized in that: The amount of bis(trifluoroacetoxyiodobenzene) PIFA added to the Spiro-OMeTAD mixed solution is 1-3 mg / mL.

7. The method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer in a perovskite solar cell according to claim 1, characterized in that: The thickness of the electron transport layer SnO2 is 80-100 nm, the thickness of the perovskite active layer is 500-700 nm, and the thickness of the hole transport layer is 110-130 nm.

8. The method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer in a perovskite solar cell according to claim 1 or 7, characterized in that: The perovskite active layer material is FAPbI3, FA 1-x Cs x PbI, MAPbI3 or FA 1- z Cs z PbI x Br y Cl 3-x-y ; Among them, x=0~3, y=0~3, z=0~3.

9. The method for solvent-assisted rapid oxidation of a Spiro-OMeTAD layer in a perovskite solar cell according to claim 1 or 7, characterized in that: The metal is gold or silver.