Photosensitive multilayer resin film, printed wiring board, semiconductor package, and method for manufacturing printed wiring board
By using a photosensitive multilayer resin film with a compound with an ethylenically unsaturated group and a thermosetting resin in a printed wiring board, combined with ultraviolet irradiation and heating curing technology, the problems of insufficient dielectric characteristics and reduced conductor adhesion are solved, and the problem of achieving the effect of achieving the Efficient interlayer insulating layer formation.
Patent Information
- Application Number
- CN202380030746.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-22
AI Technical Summary
The existing printed wiring board has the problem of insufficient dielectric characteristics in high-frequency signal transmission, and the photosensitive resin film contains fluorine-containing resin, which leads to a decrease in conductor adhesion, making it difficult to take into account both excellent dielectric characteristics and conductor adhesion.
Using a photosensitive multilayer resin film with an ethylenically unsaturated compound, a thermosetting resin, a photopolymerization initiator and an inorganic filler material, cured by ultraviolet irradiation and heating, and roughening treatment is performed to form a conductor with excellent dielectric properties and conductors. Adhesive interlayer insulating layer.
An interlayer insulating layer that maintains conductor adhesion while improving dielectric characteristics is realized, and is suitable for the manufacturing of high-density semiconductor packaging and printed wiring boards.
Smart Images

Figure BDA0005061637570000101 
Figure BDA0005061637570000102 
Figure BDA0005061637570000111
Abstract
Description
Technical Field
[0001] The present disclosure relates to a photosensitive multilayer resin film, a printed wiring board, a semiconductor package, and a method for producing the printed wiring board. Background Art
[0002] In recent years, electronic devices have been miniaturized and improved in performance, and printed wiring boards have been increasingly densified due to the increase in the number of circuit layers and the miniaturization of wiring. In particular, semiconductor packages such as BGA (ball grid array) and CSP (chip size package) equipped with semiconductor chips have become more and more dense. Therefore, printed wiring boards require not only miniaturization of wiring, but also thinning of interlayer insulation layers and reduction in the diameter of through holes used for interlayer connections.
[0003] As a method for manufacturing a printed wiring board that has been used in the past, there can be cited a method for manufacturing a multilayer printed wiring board based on a build-up method (for example, see Patent Document 1) in which an interlayer insulating layer and a conductor circuit layer are stacked in sequence. In a multilayer printed wiring board, as circuits become more miniaturized, a semi-additive method for forming circuits by plating has become the mainstream. In the conventional semi-additive method, a thermosetting resin film is used to form an interlayer insulating layer.
[0004] Laser processing is the mainstream method for forming through holes in an interlayer insulating layer formed of a thermosetting resin film. However, the reduction in the diameter of through holes using laser processing is reaching its limit. In addition, in the formation of through holes based on laser processing, each through hole needs to be formed one by one. Therefore, in the case where a plurality of through holes need to be formed due to high density, the formation of the through holes requires a lot of time, resulting in high manufacturing costs and poor manufacturing efficiency.
[0005] Under such circumstances, a method of collectively forming a plurality of small-diameter through-holes by photolithography using a photosensitive resin film has been proposed (for example, refer to Patent Document 2).
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 7-304931
[0009] Patent Document 2: Japanese Patent Application Publication No. 2017-116652 Summary of the invention
[0010] Problems to be solved by the invention
[0011] However, in recent years, the signals used in electronic devices have been increasingly being transmitted at higher speeds and higher capacities. As a result, printed wiring board substrate materials are required to have dielectric properties that can reduce the transmission loss of high-frequency signals [hereinafter sometimes referred to as "high-frequency properties"]. That is, low relative dielectric constant and low dielectric loss tangent.
[0012] In order to improve the dielectric properties of the substrate material, the inventors have studied the use of a fluorine-containing resin with a low relative dielectric constant in the photosensitive resin film used to form the interlayer insulating layer. However, if the photosensitive resin film is simply made to contain a fluorine-containing resin, even if the relative dielectric constant of the interlayer insulating layer can be reduced, the adhesion of the conductor, especially the bonding strength with the copper plating layer, will also be reduced. Therefore, it is difficult to achieve both excellent dielectric properties and conductor adhesion.
[0013] In view of such a situation, an object of the present embodiment is to provide a photosensitive multilayer resin film capable of forming an interlayer insulating layer having excellent dielectric properties and conductor adhesion, a printed wiring board using the photosensitive multilayer resin film, a method for producing the same, and a semiconductor package.
[0014] Means for solving problems
[0015] The present inventors have studied to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by the present embodiment described below.
[0016] That is, this embodiment relates to the following [1] to
[14] .
[0017] [1] A photosensitive multilayer resin film comprising a first resin composition layer and a second resin composition layer,
[0018] The first resin composition layer and the second resin composition layer respectively contain: (A) a compound having an ethylenically unsaturated group, (B) a thermosetting resin, (C) a photopolymerization initiator, and (D) an inorganic filler.
[0019] The photosensitive multilayer resin film is irradiated with 2 J / cm 2 After being exposed to ultraviolet rays, it was heated at 170°C for 1 hour to cure, and then,
[0020] The weight loss when the roughening treatment is performed under the following roughening treatment conditions in a state where the surface of the first resin composition layer is exposed and the surface of the second resin composition layer is not exposed is defined as a,
[0021] When the weight loss amount when the roughening treatment is performed under the following roughening treatment conditions in a state where the surface of the second resin composition layer is exposed and the surface of the first resin composition layer is not exposed is defined as b,
[0022] a is less than b, and a is less than or equal to 10g / m 2 .
[0023] (Conditions of Roughening Treatment)
[0024] The roughened object was immersed in a swelling solution at 70° C. for 5 minutes, then immersed in an oxidizing agent solution at 80° C. for 15 minutes, and further immersed in a neutralizing solution at 50° C. for 5 minutes, and then dried.
[0025] [2] The photosensitive multilayer resin film according to [1] above, wherein the first resin composition layer and the second resin composition layer each contain a compound having an ethylenically unsaturated group and an acidic substituent as the (A) compound having an ethylenically unsaturated group.
[0026] [3] A photosensitive multilayer resin film as described in [1] or [2] above, wherein the first resin composition layer and the second resin composition layer each contain one or more selected from the group consisting of epoxy resin, maleimide resin, allyl resin and vinyl resin as the above-mentioned (B) thermosetting resin.
[0027] [4] A photosensitive multilayer resin film as described in [3] above, wherein the first resin composition layer and the second resin composition layer each contain an epoxy resin as the (B) thermosetting resin, and the content of the epoxy resin in the first resin composition layer, calculated on a mass basis, is greater than the content of the epoxy resin in the second resin composition layer, calculated on a mass basis.
[0028] [5] The photosensitive multilayer resin film as described in any one of [1] to [4] above, wherein the first resin composition layer contains silicon dioxide as the (D) inorganic filler, and the content of the silicon dioxide in the first resin composition layer is 5 to 70% by mass.
[0029] [6] The photosensitive multilayer resin film according to any one of [1] to [5] above, wherein the second resin composition layer contains a true density of less than or equal to 1,500 kg / m 3 Silica is used as (D) inorganic filler.
[0030] [7] The photosensitive multilayer resin film as described in any one of [1] to [6] above, wherein the second resin composition layer further contains (E) a fluorine-containing resin, and the content of the (E) fluorine-containing resin is 10 to 70% by mass based on the total amount of the resin components in the second resin composition layer.
[0031] [8] The photosensitive multilayer resin film according to any one of [1] to [7] above, wherein each of the first resin composition layer and the second resin composition layer further contains (F) an elastomer.
[0032] [9] The photosensitive multilayer resin film according to any one of [1] to [8] above, wherein the content of the inorganic filler (D) in the second resin composition layer is less than 60% by mass.
[0033]
[10] A photosensitive multilayer resin film as described in any one of [1] to [9] above, wherein the layer formed by curing the first resin composition layer is a layer having a circuit pattern formed by copper plating, and the second resin composition layer is a layer having a surface to be adhered when the photosensitive multilayer resin film is stacked.
[0034]
[11] The photosensitive multilayer resin film according to any one of [1] to
[10] above, which is used for forming an interlayer insulating layer having optical through holes.
[0035]
[12] A printed wiring board having an interlayer insulating layer which is a cured product of the photosensitive multilayer resin film according to any one of [1] to
[11] above.
[0036]
[13] A semiconductor package comprising the printed wiring board described in
[12] above.
[0037]
[14] A method for manufacturing a printed wiring board, comprising the following (1) to (4).
[0038] (1): The photosensitive multilayer resin film according to any one of the above [1] to
[11] is laminated on one or both surfaces of a circuit board in a state where the second resin composition layer is the pasting surface.
[0039] (2): The photosensitive multilayer resin film laminated in the above (1) is exposed and developed to form an interlayer insulating layer having a through hole.
[0040] (3): The interlayer insulating layer having the through-hole is heated and cured.
[0041] (4): A circuit pattern is formed on the layer formed by curing the first resin composition layer of the interlayer insulating layer.
[0042] Effects of the Invention
[0043] According to the present embodiment, a photosensitive multilayer resin film capable of forming an interlayer insulating layer having excellent dielectric properties and conductor adhesion, a printed wiring board using the photosensitive multilayer resin film, a method for manufacturing the same, and a semiconductor package can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] [Figure 1 ] is a schematic diagram showing one method of manufacturing a printed wiring board using the photosensitive multilayer resin film of the present embodiment as a material for an interlayer insulating layer. DETAILED DESCRIPTION
[0045] In the numerical range described in this specification, the lower limit and upper limit of the numerical range can be replaced by the values shown in the embodiments. In addition, the lower limit and upper limit of the numerical range can be arbitrarily combined with the lower limit or upper limit of other numerical ranges. In the expression of the numerical range "AA to BB", the numerical values AA and BB at both ends are included in the numerical range as the lower limit and upper limit, respectively.
[0046] In this specification, for example, a statement such as "greater than or equal to 10" refers to 10 and a value greater than 10, and this shall prevail even if the values are different. In addition, for example, a statement such as "less than or equal to 10" refers to 10 and a value less than 10, and this shall prevail even if the values are different.
[0047] In the present specification, when there are plural substances corresponding to each component, the content of each component refers to the total content of the plural substances unless otherwise specified.
[0048] In this specification, "solid content" refers to non-volatile components other than volatile substances such as solvents. That is, "solid content" refers to components that remain when the resin composition is dried without evaporation, and also includes components that are liquid, syrupy, and waxy at room temperature. Here, in this specification, room temperature refers to 25°C.
[0049] In the present specification, the "ring carbon number" refers to the number of carbon atoms required to form a ring, and does not include the number of carbon atoms of substituents possessed by the ring. For example, the number of ring carbon atoms of a cyclohexane skeleton and a methylcyclohexane skeleton are both 6.
[0050] The expression "(meth)acrylate XX ester" refers to one or both of acrylate XX ester and the corresponding methacrylate XX ester. In addition, "(meth)acryloyl group" refers to one or both of acryloyl group and methacryloyl group.
[0051] In this specification, when a "layer" such as an interlayer insulating layer is expressed as a "layer", in addition to a solid layer, a layer in which a part is not a solid layer but is island-shaped, a layer with holes, and a layer in which the interface with the adjacent layer is unclear are also included in the "layer".
[0052] The action mechanism described in this specification is a guess, and does not limit the mechanism by which the effects of the present embodiment are achieved.
[0053] Any combination of the matters described in this specification is also included in this embodiment.
[0054] [Photosensitive multilayer resin film]
[0055] The photosensitive multilayer resin film of the present embodiment comprises a first resin composition layer and a second resin composition layer, wherein the first resin composition layer and the second resin composition layer respectively contain (A) a compound having an ethylenically unsaturated group, (B) a thermosetting resin, (C) a photopolymerization initiator, and (D) an inorganic filler.
[0056] The photosensitive multilayer resin film is irradiated with 2 J / cm 2 After being exposed to ultraviolet rays, the first resin composition layer is heated at 170° C. for 1 hour to cure, and then, the weight loss when the roughening treatment is performed under the following roughening treatment conditions in a state where the surface of the first resin composition layer is exposed and the surface of the second resin composition layer is not exposed is set as a, and the weight loss when the roughening treatment is performed under the following roughening treatment conditions in a state where the surface of the second resin composition layer is exposed and the surface of the first resin composition layer is not exposed is set as b, a is less than b, and a is less than or equal to 10 g / m 2 .
[0057] (Conditions of Roughening Treatment)
[0058] The roughened object was immersed in a swelling solution at 70° C. for 5 minutes, then immersed in an oxidizing agent solution at 80° C. for 15 minutes, and further immersed in a neutralizing solution at 50° C. for 5 minutes, and then dried.
[0059] In addition, in this specification, each component may be appropriately abbreviated as "(A) component", "(B) component" or the like.
[0060] In the following description, the photosensitive multilayer resin film may be irradiated with 2 J / cm 2 A film cured by heating at 170°C for 1 hour after being exposed to ultraviolet rays is referred to as a “cured film”, and the weight loss a when the roughening treatment is performed in a state where the surface of the above-mentioned first resin composition layer is exposed and the surface of the above-mentioned second resin composition layer is not exposed is referred to as “the weight loss a of the first surface”, and the weight loss b when the roughening treatment is performed in a state where the surface of the above-mentioned second resin composition layer is exposed and the surface of the above-mentioned first resin composition layer is not exposed is referred to as “the weight loss b of the second surface”.
[0061] The first resin composition layer and the second resin composition layer of the photosensitive multilayer resin film of the present embodiment can form a pattern such as a through hole by exposure and development. Therefore, the photosensitive multilayer resin film of the present embodiment is suitable for forming an interlayer insulating layer having a light through hole. It should be noted that in this specification, "light through hole" refers to a through hole formed by photolithography, that is, exposure and development.
[0062] The weight loss a of the first surface, which is the surface of the first resin composition layer, is lower than the weight loss b of the second surface, which is the surface of the second resin composition layer. Thus, the layer formed by curing the first resin composition layer exhibits high bonding strength with the copper plating layer.
[0063] The reason is presumed to be as follows. It is believed that the weight loss a of the first surface is lower than the weight loss b of the second surface, indicating that the dissolution of the resin caused by the roughening treatment is small on the surface of the first resin composition layer. Therefore, it is believed that even after the roughening treatment step before forming the copper plating layer, the layer formed by curing the first resin composition layer has a large amount of resin that contributes to the adhesion to the copper plating layer on the surface, and as a result, a high bonding strength with the copper plating layer is exhibited on the surface.
[0064] As described above, in the photosensitive multilayer resin film of the present embodiment, the layer formed by curing the first resin composition layer exhibits high bonding strength with the copper plating layer, and thus can improve dielectric properties while maintaining excellent conductor adhesion.
[0065] As described above, the photosensitive multilayer resin film of the present embodiment has a first resin composition layer showing high bonding strength with the copper plating layer and a second resin composition layer showing excellent dielectric properties, so that an interlayer insulating layer having excellent dielectric properties and conductor adhesion can be formed. From the viewpoint of fully exhibiting this effect, in the photosensitive multilayer resin film of the present embodiment, it is preferred that the layer formed by curing the first resin composition layer is a layer forming a circuit pattern by copper plating, and the second resin composition layer is a layer having a surface to be pasted when the photosensitive multilayer resin film is stacked.
[0066] The thickness of the first resin composition layer is not particularly limited, but is preferably 0.1 to 50 μm, more preferably 0.5 to 30 μm, and even more preferably 1 to 10 μm from the viewpoint of achieving a better balance between dielectric properties and conductor adhesion.
[0067] The thickness of the second resin composition layer is not particularly limited, but is preferably 1 to 100 μm, more preferably 3 to 50 μm, and even more preferably 5 to 40 μm from the viewpoint of achieving a better balance between dielectric properties and conductor adhesion.
[0068] The thickness of the entire photosensitive multilayer resin film of the present embodiment is not particularly limited, and may be, for example, 2 μm to 110 μm, 4 μm to 60 μm, or 7 μm to 50 μm.
[0069] <Weight reduction after roughening>
[0070] In the photosensitive multilayer resin film of the present embodiment, the weight reduction amount a of the first surface is smaller than the weight reduction amount b of the second surface.
[0071] From the viewpoint of forming an interlayer insulating layer with better dielectric properties and conductor adhesion, the weight reduction a of the first surface is less than or equal to 10 g / m 2 , preferably 0.1 to 3.3 g / m 2 , more preferably 0.5 to 3.0 g / m 2 , more preferably 0.8 to 2.7 g / m 2 .
[0072] The weight reduction b of the second surface is not particularly limited as long as it is higher than the weight reduction a of the first surface. From the viewpoint of forming an interlayer insulating layer with better dielectric properties and conductor adhesion, it is preferably 2.5 to 5.0 g / m2 within a range higher than the weight reduction a of the first surface. 2 , more preferably 2.7 to 4.5 g / m 2 , more preferably 3.0 to 4.0 g / m 2 .
[0073] From the viewpoint of forming an interlayer insulating layer with better dielectric properties and conductor adhesion, the ratio of the weight reduction a of the first surface to the weight reduction b of the second surface [a / b] is less than 1 in terms of mass ratio, preferably 0.05 to 0.95, more preferably 0.1 to 0.9, and further preferably 0.2 to 0.8.
[0074] The weight reductions a and b are measured by the above-mentioned method, and more specifically, can be measured by the method described in Examples.
[0075] For example, the weight loss a of the first surface can be made lower than the weight loss b of the second surface by making the content of the (D) inorganic filler in the first resin composition layer higher than the (D) inorganic filler in the second resin composition layer, or by making the content of the (E) fluorine-containing resin in the first resin composition layer lower than the (E) fluorine-containing resin in the second resin composition layer.
[0076] Hereinafter, each component contained in the first resin composition layer and the second resin composition layer will be described.
[0077] In the following description of components (A) to (I), in the description of preferred embodiments of components that can be contained in both the first resin composition layer and the second resin composition layer, unless otherwise specified, they are common to the first resin composition layer and the second resin composition layer.
[0078] In addition, among the following (A) to (I) components, the components contained in both the first resin composition layer and the second resin composition layer may be the same or different. That is, for example, the (A) component contained in the first resin composition layer and the (A) component contained in the second resin composition layer may be the same or different. The same applies to the (B) to (I) components.
[0079] <(A) Compound Having Ethylenically Unsaturated Group>
[0080] (A) The component is not particularly limited as long as it is a compound having an ethylenically unsaturated group.
[0081] (A) The component may be used alone or in combination of two or more.
[0082] (A) The component is a compound that exhibits photopolymerization, particularly radical polymerization, due to having an ethylenically unsaturated group.
[0083] It should be noted that, in the present specification, "ethylenically unsaturated group" refers to a substituent containing an ethylenically unsaturated bond. In addition, "ethylenically unsaturated bond" refers to a carbon-carbon double bond that can undergo an addition reaction, and does not include a double bond of an aromatic ring.
[0084] Examples of the ethylenically unsaturated group include a vinyl group, an allyl group, a (meth)acryloyl group, a propargyl group, a butenyl group, an ethynyl group, a phenylethynyl group, a maleimide group, and a nadicimide group. Among them, a (meth)acryloyl group is preferred from the viewpoint of reactivity.
[0085] From the viewpoint of being able to perform alkali development, the first resin composition layer and the second resin composition layer each preferably contain (A1) a compound having an ethylenically unsaturated group and an acidic substituent, and from the viewpoint of forming an interlayer insulating layer having better heat resistance and dielectric properties, it is preferred to contain (A2) a monomer having two or more ethylenically unsaturated groups together with the (A1) component. Components (A1) and (A2) are described below.
[0086] <(A1) Compound Having an Ethylenically Unsaturated Group and an Acidic Substituent>
[0087] Examples of the acidic substituent that the component (A1) has include a carboxyl group, a sulfonic acid group, and a phenolic hydroxyl group. Among these, a carboxyl group is preferred from the viewpoint of resolution.
[0088] The acid value of the component (A1) is not particularly limited, but is preferably 20 to 200 mgKOH / g, more preferably 40 to 180 mgKOH / g, and even more preferably 70 to 150 mgKOH / g.
[0089] When the acid value of the component (A1) is equal to or greater than the above lower limit, the alkali developability tends to be better. When the acid value of the component (A1) is equal to or less than the above upper limit, the relative dielectric constant tends to be better.
[0090] In addition, the acid value of (A1) component can be measured by the method described in Examples.
[0091] The weight average molecular weight (Mw) of the component (A1) is not particularly limited, but is preferably 600 to 30,000, more preferably 800 to 20,000, further preferably 1,000 to 10,000, and particularly preferably 1,200 to 4,000.
[0092] When the weight average molecular weight (Mw) of the component (A1) is within the above range, an interlayer insulating layer having better bonding strength with the copper plating layer, heat resistance, and insulation reliability tends to be formed.
[0093] In addition, in this specification, the weight average molecular weight (Mw) is a value calculated|required by the gel permeation chromatography (GPC) method using tetrahydrofuran as a solvent and standard polystyrene conversion, More specifically, it is a value measured by the method described in an Example.
[0094] From the viewpoint of lowering the relative dielectric constant and the dielectric loss tangent, the component (A1) preferably contains an alicyclic skeleton.
[0095] As the alicyclic skeleton possessed by the component (A1), from the viewpoint of resolution and dielectric properties, an alicyclic skeleton having 5 to 20 ring carbon atoms is preferred, an alicyclic skeleton having 5 to 18 ring carbon atoms is more preferred, an alicyclic skeleton having 6 to 16 ring carbon atoms is further preferred, an alicyclic skeleton having 7 to 14 ring carbon atoms is particularly preferred, and an alicyclic skeleton having 8 to 12 ring carbon atoms is most preferred.
[0096] From the viewpoint of resolution and dielectric properties, the alicyclic skeleton possessed by the component (A1) is preferably composed of 2 or more rings, more preferably composed of 2 to 4 rings, and further preferably composed of 3 rings. Examples of the alicyclic skeleton composed of 2 or more rings include a norbornane skeleton, a decalin skeleton, a bicycloundecane skeleton, and a saturated dicyclopentadiene skeleton. Among them, from the viewpoint of resolution and dielectric properties, a saturated dicyclopentadiene skeleton is preferred.
[0097] From the same viewpoint, the component (A1) preferably includes an alicyclic skeleton represented by the following general formula (A1-1).
[0098] [Chemistry 1]
[0099]
[0100] (Where R A1 represents an alkyl group having 1 to 12 carbon atoms, which may be substituted at any position of the above-mentioned alicyclic skeleton. 1 is an integer from 0 to 6. * represents a bonding site. )
[0101] In the above general formula (A1-1), R A1 Examples of the alkyl group having 1 to 12 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, etc. The alkyl group is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and still more preferably a methyl group.
[0102] In the above general formula (A1-1), m 1 It is an integer of 0 to 6, preferably an integer of 0 to 2, and more preferably 0. m 1 When it is an integer from 2 to 6, multiple R A1 They may be the same or different. A1 The substitutions may be made on the same carbon atom or on different carbon atoms within the possible range.
[0103] In the above general formula (A1-1), * is a bonding site with other structures.
[0104] The single bond having the bonding site * may be bonded to any carbon atom on the alicyclic skeleton, and preferably to the carbon atom represented by either 1 or 2 and the carbon atom represented by either 3 or 4 in the following general formula (A1-1').
[0105] [Chemistry 2]
[0106]
[0107] (Where R A1 、m 1 and * are the same as those in the above general formula (A1-1).
[0108] The component (A1) is preferably a compound obtained by reacting a compound obtained by reacting (a1) an epoxy resin with (a2) a (meth)acryloyl group-containing organic acid and (a3) a saturated or unsaturated group-containing polybasic acid anhydride.
[0109] In the following description, a compound obtained by reacting (a1) an epoxy resin and (a2) a (meth)acryloyl group-containing organic acid may be referred to as "component (A')".
[0110] In addition, the compound obtained by reacting the component (A') with the polybasic acid anhydride (a3) containing a saturated group or an unsaturated group may be referred to as an "acid-modified (meth)acryloyl group-containing epoxy resin derivative".
[0111] Hereinafter, preferred embodiments of the component (A1) will be described.
[0112] ((a1) Epoxy resin)
[0113] The (a1) epoxy resin preferably has two or more epoxy groups.
[0114] (a1) The epoxy resin may be used alone or in combination of two or more.
[0115] (a1) Epoxy resins can be classified into, for example, glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, etc. Among them, glycidyl ether type epoxy resins are preferred.
[0116] (a1) Epoxy resins can also be classified into various epoxy resins according to the difference in the main skeleton, for example, epoxy resins having an alicyclic skeleton, novolac epoxy resins, bisphenol epoxy resins, aralkyl epoxy resins, other epoxy resins, etc. Among them, epoxy resins having an alicyclic skeleton and novolac epoxy resins are preferred.
[0117] [Epoxy resin having an alicyclic skeleton]
[0118] The alicyclic skeleton of the epoxy resin having an alicyclic skeleton is described in the same manner as the alicyclic skeleton of the component (A1), and preferred aspects are also the same.
[0119] As the epoxy resin having an alicyclic skeleton, an epoxy resin represented by the following general formula (A1-2) is preferred.
[0120] [Chemistry 3]
[0121]
[0122] (Where R A1 Each independently represents an alkyl group having 1 to 12 carbon atoms, and may be substituted at any position of the alicyclic skeleton. A2 Each independently represents an alkyl group having 1 to 12 carbon atoms. 1 is an integer from 0 to 6, m 2 is an integer from 0 to 3. n is a number from 0 to 50. )
[0123] In the above general formula (A1-2), R A1 and R in the above general formula (A1-1) A1 The same, preferred embodiments are also the same. As R in the above general formula (A1-2) A2 Examples of the alkyl group having 1 to 12 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, etc. The alkyl group is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and still more preferably a methyl group.
[0124] In the above general formula (A1-2), m 1 and m in the above general formula (A1-1) 1 The same, the preferred method is also the same.
[0125] In the above general formula (A1-2), m 2 It is an integer of 0 to 3, preferably 0 or 1, and more preferably 0.
[0126] In the general formula (A1-2), n represents the number of structural units in parentheses, and is a number from 0 to 50. Usually, epoxy resins are mixtures of substances having different numbers of structural units in parentheses, and in this case, n is represented by the average value of the mixture. As n, a number of 0 to 30 is preferred.
[0127] As the epoxy resin having an alicyclic skeleton, a commercially available product can be used. Examples of the commercially available products include "ZXR-1807H" (trade name, manufactured by Nippon Kayaku Co., Ltd.), "XD-1000" (trade name, manufactured by Nippon Kayaku Co., Ltd.), and "EPICLON (registered trademark) HP-7200" (trade name, manufactured by DIC Corporation).
[0128] [Novolac type epoxy resin]
[0129] Examples of the novolac epoxy resin include bisphenol novolac epoxy resins such as bisphenol A novolac epoxy resin, bisphenol F novolac epoxy resin, and bisphenol S novolac epoxy resin; phenol novolac epoxy resin, cresol novolac epoxy resin, biphenyl novolac epoxy resin, and naphthol novolac epoxy resin.
[0130] As the novolac-type epoxy resin, an epoxy resin having a structural unit represented by the following general formula (A1-3) is preferred.
[0131] [Chemistry 4]
[0132]
[0133] (Where R A3Each independently represents a hydrogen atom or a methyl group, Y A1 Each independently represents a hydrogen atom or a glycidyl group. A1 At least one of them is a glycidyl group. )
[0134] From the viewpoint of resolution, R in the above general formula (A1-3) A3 Preferably, all of them are hydrogen atoms. From the same viewpoint, Y in the above general formula (A1-3) A1 Preferably, both are glycidyl groups.
[0135] The number of the structural units in the epoxy resin (a1) having the structural unit represented by the general formula (A1-3) is 1 or more, preferably 10 to 100, more preferably 13 to 80, and further preferably 15 to 70. When the number of the structural units is within the above range, there is a tendency that an interlayer insulating layer having better conductor adhesion, heat resistance, and insulation reliability can be formed.
[0136] As the epoxy resin having the structural unit represented by the general formula (A1-3), a commercially available product may be used. Examples of the commercially available product include the "EXA-7376" series (manufactured by DIC Corporation, trade name, wherein R in the general formula (A1-3) is A3 are hydrogen atoms, Y A1 are all epoxy resins containing glycidyl groups), "EPON SU8" series (manufactured by Mitsubishi Chemical Corporation, trade name, R in the above general formula (A1-3) A3 All are methyl, Y A1 are all glycidyl epoxy resins) and the like.
[0137] 〔Bisphenol type epoxy resin〕
[0138] As a bisphenol type epoxy resin, a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a bisphenol S type epoxy resin, 3,3',5,5'-tetramethyl-4,4'-diglycidyloxydiphenylmethane etc. are mentioned, for example.
[0139] 〔Aralkyl type epoxy resin〕
[0140] As an aralkyl type epoxy resin, a phenol aralkyl type epoxy resin, a biphenyl aralkyl type epoxy resin, a naphthol aralkyl type epoxy resin etc. are mentioned, for example.
[0141] 〔Other epoxy resins〕
[0142] Examples of other epoxy resins include stilbene-type epoxy resins, naphthalene-type epoxy resins, naphthylene ether-type epoxy resins, biphenyl-type epoxy resins, dihydroanthracene-type epoxy resins, cyclohexanedimethanol-type epoxy resins, trimethylol-type epoxy resins, alicyclic epoxy resins, aliphatic chain epoxy resins, heterocyclic epoxy resins, spiro-ring-containing epoxy resins, and rubber-modified epoxy resins.
[0143] ((a2) (meth)acryloyl-containing organic acid)
[0144] As the (a2) (meth)acryloyl group-containing organic acid, a (meth)acryloyl group-containing monocarboxylic acid is preferred.
[0145] Examples of the monocarboxylic acid containing a (meth)acryloyl group include acrylic acid derivatives such as acrylic acid, a dimer of acrylic acid, methacrylic acid, β-furfuryl acrylic acid, β-styryl acrylic acid, cinnamic acid, crotonic acid, and α-cyanocinnamic acid; half-ester compounds that are reaction products of hydroxyl-containing acrylic acid esters and dibasic acid anhydrides; monoglycidyl ethers containing a (meth)acryloyl group or half-ester compounds that are reaction products of monoglycidyl esters containing a (meth)acryloyl group and dibasic acid anhydrides; and the like.
[0146] The component (a2) may be used alone or in combination of two or more.
[0147] In the reaction of component (a1) and component (a2), the amount of component (a2) used is not particularly limited, but is preferably 0.6 to 1.1 equivalents, more preferably 0.8 to 1.05 equivalents, and still more preferably 0.9 to 1.02 equivalents relative to 1 equivalent of the epoxy group of component (a1). By reacting component (a1) and component (a2) at the above ratio, there is a tendency that the polymerizability of component (a1) is improved and the resolution is improved.
[0148] It is preferred that the components (a1) and (a2) are dissolved in an organic solvent and reacted while heating. In the reaction, a known reaction catalyst, polymerization inhibitor, etc. may be used as necessary.
[0149] When a monocarboxylic acid containing a (meth)acryloyl group is used as the component (a2), the component (A') obtained by reacting the components (a1) and (a2) has a hydroxyl group formed by a ring-opening addition reaction between the epoxy group of the component (a1) and the carboxyl group of the component (a2). Then, the component (A') is reacted with a polyacid anhydride containing a saturated or unsaturated group (a3), thereby obtaining an acid-modified epoxy resin derivative containing a (meth)acryloyl group, in which the hydroxyl group of the component (A') and the acid anhydride group of the component (a3) are half-esterified. It should be noted that the hydroxyl group of the component (A') may also include the hydroxyl group originally present in the component (a1).
[0150] ((a3) polyacid anhydride)
[0151] As (a3) component, it is possible to contain a saturated group or an unsaturated group. As (a3) component, for example, succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, itaconic anhydride etc. can be listed. Among them, from the viewpoint of resolution, tetrahydrophthalic anhydride is preferred. (a3) component can be used alone or in combination of two or more.
[0152] In the reaction between the components (A') and (a3), for example, by reacting 0.1 to 1.0 equivalent of the component (a3) per 1 equivalent of the hydroxyl groups in the component (A'), the acid value of the acid-modified (meth)acryloyl group-containing epoxy resin derivative can be well adjusted.
[0153] <(A2) Monomer having two or more ethylenically unsaturated groups>
[0154] The component (A2) is mainly used as a crosslinking agent for the component (A1).
[0155] The first resin composition layer and the second resin composition layer contain the component (A2) together with the component (A1), thereby increasing the crosslinking density due to the photoradical polymerization reaction, improving the alkaline developer resistance and the resolution, and tending to form an interlayer insulating layer having better heat resistance.
[0156] In addition, the component (A2) may or may not have an acidic substituent.
[0157] The number of ethylenically unsaturated groups possessed by component (A2) is 2 or more, preferably 2 to 10, more preferably 2 to 8, and even more preferably 2 to 7 from the viewpoint of resolution and forming an interlayer insulating layer having better heat resistance and dielectric properties.
[0158] (A2) As a component, a bifunctional monomer which has two ethylenically unsaturated groups, a polyfunctional monomer which has three or more ethylenically unsaturated groups, etc. are mentioned.
[0159] Examples of the difunctional monomer having two ethylenically unsaturated groups include aliphatic di(meth)acrylates such as trimethylolpropane di(meth)acrylate, polypropylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate; di(meth)acrylates having an alicyclic skeleton such as dicyclopentadiene di(meth)acrylate and tricyclodecane dimethanol di(meth)acrylate; and aromatic di(meth)acrylates such as 2,2-bis(4-(meth)acryloyloxypolyethoxypolypropoxyphenyl)propane and bisphenol A diglycidyl ether di(meth)acrylate.
[0160] Examples of the polyfunctional monomer having three or more ethylenically unsaturated groups include (meth)acrylate compounds having a skeleton derived from trimethylolpropane, such as trimethylolpropane tri(meth)acrylate; (meth)acrylate compounds having a skeleton derived from tetramethylolmethane, such as tetramethylolmethane tri(meth)acrylate and tetramethylolmethane tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from pentaerythritol, such as pentaerythritol tri(meth)acrylate and pentaerythritol tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from dipentaerythritol, such as dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate; (meth)acrylate compounds having a skeleton derived from di(trimethylolpropane), such as di(trimethylolpropane) tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from diglycerol, and the like.
[0161] Here, the above-mentioned “(meth)acrylate compound having a skeleton derived from XXX” (wherein XXX is a compound name) refers to an esterification product of XXX and (meth)acrylic acid, and the esterification product also includes compounds modified with an alkyleneoxy group.
[0162] Among the above options, from the viewpoint of resolution and the viewpoint of forming an interlayer insulating layer with better conductor adhesion, the (A2) component is preferably a polyfunctional monomer having three or more ethylenically unsaturated groups, and more preferably a (meth)acrylate compound having a skeleton derived from trimethylolpropane or a (meth)acrylate compound having a skeleton derived from dipentaerythritol.
[0163] Component (A) may or may not contain compounds other than components (A1) and (A2). Components other than components (A1) and (A2) include, for example, monofunctional monomers having one ethylenically unsaturated group and no acidic substituent.
[0164] (Content of Component (A) in First Resin Composition Layer)
[0165] The content of the component (A) in the first resin composition layer is not particularly limited, but is preferably 10 to 80% by mass, more preferably 20 to 60% by mass, and even more preferably 30 to 50% by mass, based on the total amount of the resin components in the first resin composition layer, from the viewpoint of the resolution of the photosensitive multilayer resin film and the dielectric properties of the interlayer insulating layer to be formed.
[0166] Here, in this specification, "resin component" refers to a resin and a compound that forms a resin by a curing reaction. For example, in the photosensitive multilayer resin film of this embodiment, component (A), component (B), component (E), and component (F) are classified as resin components.
[0167] On the other hand, the resin component does not contain the (C) component, the (D) component, the (G) component, and the (H) component.
[0168] When the first resin composition layer contains the component (A1), the content of the component (A1) in the first resin composition layer is not particularly limited. From the viewpoint of resolution and dielectric properties of the formed interlayer insulating layer, it is preferably 5 to 70% by mass, more preferably 10 to 50% by mass, and even more preferably 20 to 40% by mass based on the total amount of the resin components in the first resin composition layer.
[0169] When the first resin composition layer contains the components (A1) and (A2), the content of the component (A2) in the first resin composition layer is not particularly limited. However, from the viewpoint of resolution and dielectric properties of the interlayer insulating layer to be formed, it is preferably 5 to 80 parts by mass, more preferably 10 to 60 parts by mass, and even more preferably 20 to 40 parts by mass, relative to 100 parts by mass of the component (A1) in the first resin composition layer.
[0170] (Content of Component (A) in Second Resin Composition Layer)
[0171] The content of the component (A) in the second resin composition layer is not particularly limited, but is preferably 10 to 80% by mass, more preferably 20 to 60% by mass, and even more preferably 30 to 50% by mass, based on the total amount of the resin components in the second resin composition layer, from the viewpoint of resolution and dielectric properties of the formed interlayer insulating layer.
[0172] When the second resin composition layer contains the component (A1), the content of the component (A1) in the second resin composition layer is not particularly limited. From the viewpoint of resolution and dielectric properties of the formed interlayer insulating layer, it is preferably 5 to 60% by mass, more preferably 10 to 40% by mass, and even more preferably 15 to 30% by mass based on the total amount of the resin components in the second resin composition layer.
[0173] When the second resin composition layer contains the components (A1) and (A2), the content of the component (A2) in the second resin composition layer is not particularly limited. However, from the viewpoint of resolution and dielectric properties of the interlayer insulating layer to be formed, it is preferably 20 to 100 parts by mass, more preferably 40 to 90 parts by mass, and even more preferably 60 to 80 parts by mass, relative to 100 parts by mass of the component (A1) in the second resin composition layer.
[0174] <(B) Thermosetting resin>
[0175] (B) The thermosetting resin is not particularly limited as long as it is a thermosetting resin.
[0176] When the first resin composition layer and the second resin composition layer contain the (B) thermosetting resin, the heat resistance of the interlayer insulating layer to be formed tends to be improved.
[0177] (B) Thermosetting resins may be used alone or in combination of two or more.
[0178] Examples of the thermosetting resin (B) include epoxy resins, isocyanate resins, maleimide resins, phenolic resins, cyanate resins, benzoic acid resins, Oxazine resin, oxetane resin, amino resin, unsaturated polyester resin, allyl resin, vinyl resin, dicyclopentadiene resin, silicone resin, triazine resin, melamine resin, other well-known thermosetting resins, etc.
[0179] Among the above options, from the viewpoint of forming an interlayer insulating layer with better heat resistance and conductor adhesion, the first resin composition layer and the second resin composition layer preferably contain one or more selected from the group consisting of epoxy resin, maleimide resin, allyl resin and vinyl resin as component (B), and more preferably contain epoxy resin.
[0180] Furthermore, from the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the second resin composition layer preferably further contains a maleimide resin.
[0181] (Epoxy resin)
[0182] As the epoxy resin, an epoxy resin having two or more epoxy groups is preferred.
[0183] Epoxy resins can be classified into, for example, glycidyl ether epoxy resins, glycidyl amine epoxy resins, glycidyl ester epoxy resins, etc. Among them, glycidyl ether epoxy resins are preferred.
[0184] In addition, epoxy resins can also be classified into various epoxy resins according to the difference of the main skeleton. Among the above-mentioned various types of epoxy resins, they can be further classified as follows. Specifically, epoxy resins can be classified into bisphenol-based epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, and bisphenol S epoxy resin; bisphenol A novolac epoxy resin; bisphenol F novolac epoxy resin and other bisphenol novolac epoxy resins; phenol novolac epoxy resins other than the above-mentioned bisphenol novolac epoxy resins such as phenol novolac epoxy resin, cresol novolac epoxy resin, and biphenyl novolac epoxy resin; phenol aralkyl epoxy resin; stilbene epoxy resin ; Epoxy resins containing naphthalene skeletons such as naphthol novolac type epoxy resin, naphthol type epoxy resin, naphthol aralkyl type epoxy resin, and naphthylene ether type epoxy resin; biphenyl type epoxy resin; biphenyl aralkyl type epoxy resin; benzyl dimethyl type epoxy resin; dihydroanthracene type epoxy resin; alicyclic epoxy resins such as saturated dicyclopentadiene type epoxy resin; heterocyclic epoxy resin; epoxy resin containing spiro ring; cyclohexanedimethanol type epoxy resin; trimethylol type epoxy resin; aliphatic chain epoxy resin; rubber modified epoxy resin, etc.
[0185] Among them, the epoxy resin is preferably a bisphenol epoxy resin, a naphthalene skeleton-containing epoxy resin, or a biphenyl aralkyl type epoxy resin, and more preferably an epoxy resin containing a naphthalene skeleton or a biphenyl aralkyl type epoxy resin.
[0186] (isocyanate resin)
[0187] As isocyanate resin, for example, aliphatic isocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate; alicyclic isocyanates such as 1,3-cyclopentane diisocyanate, 1,4-cyclohexane diisocyanate, 1,2-cyclohexane diisocyanate, isophorone diisocyanate, and norbornane diisocyanate; aromatic isocyanates such as xylylene diisocyanate, 2,4-toluene diisocyanate, and 2,6-toluene diisocyanate; their biuret bodies; their urate bodies, etc. Among them, aliphatic isocyanates are preferred, and hexamethylene diisocyanate is more preferred.
[0188] (Maleimide resin)
[0189] As maleimide resin, for example, aromatic maleimide compounds having N-substituted maleimide groups directly bonded to an aromatic ring, aliphatic maleimide compounds having N-substituted maleimide groups directly bonded to an aliphatic hydrocarbon group, etc. Among them, aromatic maleimide compounds are preferred, and aromatic bismaleimide compounds are more preferred, from the viewpoint of heat resistance and handling properties.
[0190] Examples of the aromatic maleimide compound include bis(4-maleimidephenyl)methane, 2,2-bis[4-(4-maleimidephenoxy)phenyl]propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, biphenyl aralkyl maleimide resins, and aromatic bismaleimide resins having an indane skeleton. Among them, aromatic bismaleimide resins having an indane skeleton are preferred.
[0191] (allyl resin)
[0192] Examples of the allyl resin include allyl isocyanurates such as diallyl isocyanurate and triallyl isocyanurate; allyl cyanurates such as diallyl cyanurate and triallyl cyanurate; 1,3,4,6-tetraallyl glycoluril, etc. Among them, allyl isocyanurates are preferred, and diallyl isocyanurate is more preferred, from the viewpoints of heat resistance, dielectric properties, and operability.
[0193] (Content of Component (B) in First Resin Composition Layer)
[0194] The content of the (B) thermosetting resin in the first resin composition layer is not particularly limited, but is preferably 10 to 90% by mass, more preferably 20 to 80% by mass, and even more preferably 30 to 70% by mass, based on the total amount of the resin components in the first resin composition layer, from the viewpoint of forming an interlayer insulating layer having better conductor adhesion and heat resistance.
[0195] When the first resin composition layer contains an epoxy resin as the (B) thermosetting resin, the content of the epoxy resin in the first resin composition layer is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better conductor adhesion and heat resistance, the content of the epoxy resin is preferably 7 to 80% by mass, more preferably 15 to 70% by mass, and even more preferably 20 to 60% by mass, based on the total amount of the resin components in the first resin composition layer.
[0196] From the viewpoint of forming an interlayer insulating layer having better conductor adhesion, the content of the epoxy resin by mass in the first resin composition layer is preferably larger than the content of the epoxy resin by mass in the second resin composition layer.
[0197] When the first resin composition layer contains an isocyanate resin as the (B) thermosetting resin, the content of the isocyanate resin in the first resin composition layer is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better conductor adhesion and heat resistance, the content is preferably 1 to 30% by mass, more preferably 3 to 20% by mass, and even more preferably 5 to 15% by mass, based on the total amount of the resin components in the first resin composition layer.
[0198] (Content of Component (B) in Second Resin Composition Layer)
[0199] The content of the (B) thermosetting resin in the second resin composition layer is not particularly limited, but is preferably 1 to 50% by mass, more preferably 10 to 40% by mass, and even more preferably 20 to 30% by mass, based on the total amount of the resin components in the second resin composition layer, from the viewpoint of forming an interlayer insulating layer having better heat resistance and dielectric properties.
[0200] When the second resin composition layer contains an epoxy resin as the (B) thermosetting resin, the content of the epoxy resin in the second resin composition layer is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and dielectric properties, the content is preferably 1 to 50% by mass, more preferably 5 to 30% by mass, and even more preferably 7 to 15% by mass, based on the total amount of the resin components in the second resin composition layer.
[0201] When the second resin composition layer contains an isocyanate resin as the (B) thermosetting resin, the content of the isocyanate resin in the second resin composition layer is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and dielectric properties, the content is preferably 1 to 20% by mass, more preferably 2 to 15% by mass, and even more preferably 4 to 10% by mass, based on the total amount of the resin components in the second resin composition layer.
[0202] When the second resin composition layer contains a maleimide resin as the (B) thermosetting resin, the content of the maleimide resin in the second resin composition layer is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and dielectric properties, the content is preferably 1 to 40% by mass, more preferably 3 to 30% by mass, and even more preferably 5 to 20% by mass, based on the total amount of the resin components in the second resin composition layer.
[0203] <(C) Photopolymerization Initiator>
[0204] (C) The photopolymerization initiator is a polymerization initiator that mainly initiates the photoradical polymerization reaction of the ethylenically unsaturated group contained in the component (A).
[0205] The first resin composition layer and the second resin composition layer tend to have a further improved resolution by containing the (C) photopolymerization initiator.
[0206] (C) The photopolymerization initiator may be used alone or in combination of two or more.
[0207] (C) The photopolymerization initiator includes, for example, benzoin compounds such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; acetophenone compounds such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-[4-(methylthio)benzoyl]-2-(4-morpholino)propane, and N,N-dimethylaminoacetophenone; anthraquinone compounds such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; ketal compounds such as acetophenone dimethyl ketal and benzyl dimethyl ketal; 9-phenylacridine, 1- ,7-bis(9,9'-acridinyl)heptane and other acridinium compounds; phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide and other acylphosphine oxide compounds; 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyl oxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanone 1-(O-acetyl oxime) , 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime] and other oxime ester compounds; 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone and other thioxanthone compounds; 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone and other benzophenone compounds, etc. Among them, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanone 1-(O-acetyloxime) are preferred.
[0208] (Content of Component (C) in First Resin Composition Layer)
[0209] The content of the (C) photopolymerization initiator in the first resin composition layer is not particularly limited, but is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the (A) component in the first resin composition layer, from the viewpoint of easily obtaining a moderate polymerization reaction promotion effect.
[0210] (Content of Component (C) in Second Resin Composition Layer)
[0211] The content of the (C) photopolymerization initiator in the second resin composition layer is not particularly limited, but is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the (A) component in the second resin composition layer, from the viewpoint of easily obtaining a moderate polymerization reaction promotion effect.
[0212] <(D) Inorganic filler>
[0213] When the first resin composition layer and the second resin composition layer contain the (D) inorganic filler, the interlayer insulating layer formed tends to have further improved low thermal expansion, heat resistance, and flame retardancy.
[0214] (D) The inorganic filler may be used alone or in combination of two or more.
[0215] In the photosensitive multilayer resin film of the present embodiment, the first resin composition layer preferably contains silicon dioxide as the (D) inorganic filler. Thereby, the layer formed by curing the first resin composition layer exhibits high bonding strength with the copper plating layer.
[0216] In addition, the second resin composition layer preferably contains silicon dioxide from the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, and flame retardancy.
[0217] Silica may be surface-treated with a coupling agent such as a silane coupling agent.
[0218] As silica, for example, precipitated silica with high water content produced by a wet process, dry process silica produced by a dry process and containing almost no bound water, etc., etc. can be cited. In addition, as dry process silica, for example, crushed silica, fumed silica, fused silica, etc. can also be cited depending on the production method.
[0219] Examples of silica include (D1) having a true density of more than 1,500 kg / m 3 Silica (hereinafter also referred to as "(D1) component"), (D2) true density less than or equal to 1,500 kg / m 3 Silicon dioxide (hereinafter also referred to as "(D2) component") and the like.
[0220] The component (D1) tends to have a low dielectric loss tangent. Therefore, from the viewpoint of forming an interlayer insulating layer having more excellent dielectric properties, the first resin composition layer preferably contains the component (D1).
[0221] From the viewpoint of low thermal expansion, the true density of silica as the component (D1) is preferably greater than 1,500 and less than or equal to 2,200 kg / m 3 , more preferably 1,600 to 2,200 kg / m 3 , more preferably 1,800 to 2,200 kg / m 3 .
[0222] The component (D2) tends to have a small relative dielectric constant. Therefore, from the viewpoint of forming an interlayer insulating layer having more excellent dielectric properties, the second resin composition layer preferably contains the component (D2).
[0223] From the viewpoint of dielectric properties, the true density of silicon dioxide as the component (D2) is preferably 1,000 to 1,500 kg / m 3 , more preferably 1,100 to 1,500 kg / m 3 , more preferably 1,200 to 1,500 kg / m 3 , particularly preferably 1,250 to 1,450 kg / m 3 , most preferably 1,250 to 1,400 kg / m 3 .
[0224] In addition, the true density of silica can be measured using a dry type automatic density meter "AccuPycII 1340" (manufactured by Shimadzu Corporation).
[0225] Examples of the (D) inorganic filler other than silica include alumina, titanium oxide, mica, beryllium oxide, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay, talc, aluminum borate, and silicon carbide.
[0226] (D) Volume average particle size of the inorganic filler (D 50 ) is not particularly limited, but from the viewpoint of resolution, it is preferably 0.01 to 3.0 μm, more preferably 0.1 to 2.5 μm, and even more preferably 0.3 to 2.0 μm.
[0227] It should be noted that in this specification, the volume average particle size (D 50 ) can be determined as follows: using a submicron particle analyzer (manufactured by Beckman Coulter, Ltd., trade name: N5), in accordance with international standard ISO13321, particles dispersed in a solvent are measured with a refractive index of 1.38, and the particle size is determined as the particle size equivalent to the cumulative value of 50% (volume basis) in the particle size distribution.
[0228] (Content of (D) Inorganic Filler in First Resin Composition Layer)
[0229] The content of the (D) inorganic filler in the first resin composition layer is not particularly limited, but is preferably 5 to 70% by mass, more preferably 15 to 60% by mass, and even more preferably 25 to 50% by mass, from the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, flame retardancy, and better conductor adhesion.
[0230] When the first resin composition layer contains silica, the content of silica in the first resin composition layer is not particularly limited, but is preferably 5 to 70% by mass, more preferably 15 to 60% by mass, and further preferably 25 to 50% by mass, from the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, flame retardancy and better conductor adhesion.
[0231] From the viewpoint of forming an interlayer insulating layer having better conductor adhesion, the content of silicon dioxide by mass in the first resin composition layer is preferably larger than the content of silicon dioxide by mass in the second resin composition layer.
[0232] When the first resin composition layer contains the component (D1), the content of the component (D1) in the first resin composition layer is not particularly limited. From the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, flame retardancy and better conductor adhesion, the content is preferably 60 to 100 mass %, more preferably 70 to 100 mass %, and even more preferably 80 to 100 mass % relative to the total amount (100 mass %) of the (D) inorganic filler in the first resin composition layer.
[0233] (Content of (D) Inorganic Filler in Second Resin Composition Layer)
[0234] The content of the (D) inorganic filler in the second resin composition layer is not particularly limited, but is preferably less than 60% by mass, more preferably 1 to 55% by mass, further preferably 2 to 50% by mass, further preferably 3 to 30% by mass, and particularly preferably 5 to 20% by mass, from the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance and flame retardancy.
[0235] When the second resin composition layer contains silica, the content of silica in the second resin composition layer is not particularly limited, but is preferably less than 60% by mass, more preferably 1 to 55% by mass, further preferably 2 to 50% by mass, further preferably 3 to 30% by mass, and particularly preferably 5 to 20% by mass, from the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, flame retardancy and better conductor adhesion.
[0236] When the second resin composition layer contains the component (D2), the content of the component (D2) in the second resin composition layer is not particularly limited. From the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance and flame retardancy, the content is preferably 60 to 100% by mass, more preferably 70 to 100% by mass, and even more preferably 80 to 100% by mass, relative to the total amount (100% by mass) of the component (D) in the second resin composition layer.
[0237] <(E) Fluorine-containing resin>
[0238] In the photosensitive multilayer resin film of the present embodiment, it is preferred that the second resin composition layer further contains (E) a fluorine-containing resin. Thereby, the interlayer insulating layer formed of the photosensitive multilayer resin film of the present embodiment tends to have a low relative dielectric constant.
[0239] (E) The fluorine-containing resin may be used alone or in combination of two or more.
[0240] (E) Examples of the fluorine-containing resin include polymers of olefins containing fluorine atoms (hereinafter also referred to as "fluorine-containing olefins").
[0241] The fluorine-containing olefin may be one in which a part of hydrogen atoms in carbon-hydrogen bonds are substituted with fluorine atoms, but preferably one in which all hydrogen atoms in carbon-hydrogen bonds are substituted with fluorine atoms from the viewpoint of further reducing the relative dielectric constant.
[0242] (E) The fluorine-containing resin includes, for example, polymonofluoroethylene, polydifluoroethylene, polytrifluoroethylene, polytetrafluoroethylene, polyhexafluoropropylene, polyvinyl fluoride, polyvinylidene fluoride, etc. Among them, polytetrafluoroethylene is preferred.
[0243] (E) The fluorine-containing resin is preferably in the form of particles.
[0244] The volume average particle size (D) of the fluorine-containing resin (E) as particles 50 ) is not particularly limited, but from the viewpoint of resolution, it is preferably 0.01 μm to 3.0 μm, more preferably 0.05 μm to 2.5 μm, and further preferably 0.1 μm to 2.0 μm.
[0245] (Content of component (E) in first resin composition layer)
[0246] The first resin composition layer may contain (E) a fluorine-containing resin, but preferably contains no (E) fluorine-containing resin from the viewpoint of resolution and from the viewpoint of forming an interlayer insulating layer having more excellent conductor adhesion.
[0247] When the first resin composition layer contains the (E) fluorine-containing resin, the content of the (E) fluorine-containing resin in the first resin composition layer is preferably as low as possible. From the same viewpoint as described above, the content is preferably 20% by mass or less, more preferably 10% by mass or less, and further preferably 1% by mass or less, based on the total amount of the resin components in the first resin composition layer.
[0248] (Content of component (E) in second resin composition layer)
[0249] The content of the (E) fluorine-containing resin in the second resin composition layer is not particularly limited, but is preferably 10 to 70% by mass, more preferably 20 to 50% by mass, and still more preferably 25 to 40% by mass, based on the total amount of the resin components in the second resin composition layer, from the viewpoint of resolution and from the viewpoint of forming an interlayer insulating layer having better insulation reliability, relative dielectric constant, heat resistance and conductor adhesion.
[0250] <(F) Elastomer>
[0251] The first resin composition layer and the second resin composition layer may each further contain (F) an elastomer.
[0252] When the first resin composition layer and the second resin composition layer contain the (F) elastomer, the interlayer insulating layer formed tends to have further improved conductor adhesion.
[0253] It should be noted that the “elastomer” herein refers to a polymer having a glass transition temperature of 25° C. or less as measured by differential scanning calorimetry in accordance with JIS K 6240:2011.
[0254] (F) The elastomer may be used alone or in combination of two or more.
[0255] (F) Examples of the elastomer include polybutadiene elastomers, polyester elastomers, styrene elastomers, olefin elastomers, urethane elastomers, polyamide elastomers, acrylic elastomers, silicone elastomers, and derivatives of these elastomers. Among these, polybutadiene elastomers are preferred from the viewpoint of compatibility with the resin component and from the viewpoint of forming an interlayer insulating layer with better conductor adhesion.
[0256] Preferred examples of the polybutadiene-based elastomer include those containing a 1,2-vinyl group derived from 1,3-butadiene.
[0257] From the viewpoint of resolution, the polybutadiene-based elastomer is preferably a polybutadiene-based elastomer having an acid anhydride group, and more preferably a polybutadiene-based elastomer having an acid anhydride group derived from maleic anhydride.
[0258] When the polybutadiene elastomer has an acid anhydride group, the number of the acid anhydride groups in one molecule is not particularly limited, but is preferably 1 to 12, more preferably 3 to 11, and even more preferably 6 to 10 from the viewpoint of resolution and forming an interlayer insulating layer with a better relative dielectric constant.
[0259] The number average molecular weight (Mn) of the (F) elastomer is not particularly limited, but is preferably 1,000 to 100,000, more preferably 2,000 to 50,000, further preferably 3,000 to 10,000, and particularly preferably 4,000 to 7,000.
[0260] In addition, in this specification, the number average molecular weight (Mn) is a value calculated|required by the gel permeation chromatography (GPC) method using tetrahydrofuran as a solvent and standard polystyrene conversion, More specifically, it is a value measured by the method described in an Example.
[0261] (Content of component (F) in first resin composition layer)
[0262] When the first resin composition layer contains the (F) elastomer, the content of the (F) elastomer in the first resin composition layer is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content is preferably 1 to 30% by mass, more preferably 3 to 20% by mass, and even more preferably 5 to 15% by mass, based on the total amount of the resin components in the first resin composition layer.
[0263] (Content of component (F) in second resin composition layer)
[0264] When the second resin composition layer contains the (F) elastomer, the content of the (F) elastomer in the second resin composition layer is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content is preferably 0.5 to 20% by mass, more preferably 1 to 15% by mass, and even more preferably 2 to 10% by mass, based on the total amount of the resin components in the second resin composition layer.
[0265] <(G) Organic peroxide>
[0266] The first resin composition layer and the second resin composition layer each preferably further contain (G) an organic peroxide. The (G) organic peroxide is mainly a polymerization initiator for thermal radical polymerization of the ethylenically unsaturated group possessed by the component (A) and, if necessary, the component (B).
[0267] When the first resin composition layer and the second resin composition layer contain the (G) organic peroxide, the interlayer insulating layer formed tends to have further improved heat resistance, dielectric properties, and the like.
[0268] (G) The organic peroxide may be used alone or in combination of two or more.
[0269] Examples of the organic peroxide (G) include peroxyketals such as 1,1-di(tert-butylperoxy)cyclohexane, 2,2-di(tert-butylperoxy)butane, 2,2-di(4,4-di-tert-butylperoxycyclohexyl)propane, and 1,1-di(tert-amylperoxy)cyclohexane; hydroperoxides such as cumene hydroperoxide and tert-butyl hydroperoxide; alkyl peroxides such as tert-butyl peroxyacetate and tert-amyl peroxyisononanoate; tert-butyl Dialkyl peroxides such as cumyl peroxide, di-tert-butyl peroxide, dicumyl peroxide, di-tert-hexyl peroxide, and 1,3-di(tert-butylperoxyisopropyl)benzene; peroxyesters such as tert-butyl peroxyacetate, tert-butyl peroxybenzoate, and tert-butyl peroxyisopropylmonocarbonate; peroxycarbonates such as tert-butyl peroxyisopropylcarbonate and polyether tetra(tert-butylperoxycarbonate); diacyl peroxides such as dibenzoyl peroxide, etc. Among them, 1,3-di(tert-butylperoxyisopropyl)benzene is preferred.
[0270] (Content of component (G) in first resin composition layer)
[0271] When the first resin composition layer contains (G) an organic peroxide, the content of the (G) organic peroxide in the first resin composition layer is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content is preferably 0.1 to 10 parts by mass, more preferably 1 to 7 parts by mass, and even more preferably 1.5 to 4 parts by mass, relative to 100 parts by mass of the (A) component in the first resin composition layer.
[0272] (Content of component (G) in second resin composition layer)
[0273] When the second resin composition layer contains (G) an organic peroxide, the content of the (G) organic peroxide in the second resin composition layer is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content is preferably 0.1 to 10 parts by mass, more preferably 1 to 7 parts by mass, and even more preferably 1.5 to 4 parts by mass, relative to 100 parts by mass of the (A) component in the second resin composition layer.
[0274] <(H) Curing Accelerator>
[0275] It is preferred that each of the first resin composition layer and the second resin composition layer further contain (H) a curing accelerator.
[0276] When the first resin composition layer and the second resin composition layer contain the (H) curing accelerator, the interlayer insulating layer formed tends to have further improved heat resistance, dielectric properties, and the like.
[0277] (H) The curing accelerator may be used alone or in combination of two or more.
[0278] Examples of the (H) curing accelerator include imidazole compounds such as 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenylimidazole, 2-phenyl-1-benzyl-1H-imidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and isocyanate-masked imidazole (addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole); tertiary amines such as trimethylamine, N,N-dimethyloctylamine, N-benzyldimethylamine, pyridine, N-methylmorpholine, hexa(N-methyl)melamine, 2,4,6-tris(dimethylaminophenol), tetramethylguanidine, and m-aminophenol; organic phosphines such as tributylphosphine, triphenylphosphine, and tri-2-cyanoethylphosphine; tri-n-butyl(2,5-dihydroxyphenyl)bromide; Hexadecyl tributyl chloride wait Salts; quaternary ammonium salts such as benzyltrimethylammonium chloride and phenyltributylammonium chloride; the above-mentioned polyacid anhydrides; diphenyl iodide Tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, 2,4,6-triphenylthiopyran Hexafluorophosphate, etc.
[0279] Among them, imidazole compounds are preferred from the viewpoint of obtaining an excellent curing effect.
[0280] (Content of Component (H) in First Resin Composition Layer)
[0281] When the first resin composition layer contains (H) a curing accelerator, the content of the (H) curing accelerator in the first resin composition layer is not particularly limited, but is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and even more preferably 1 to 4 parts by mass, relative to 100 parts by mass of the (B) component in the first resin composition layer, from the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion.
[0282] (Content of Component (H) in Second Resin Composition Layer)
[0283] When the second resin composition layer contains (H) a curing accelerator, the content of the (H) curing accelerator in the second resin composition layer is not particularly limited, but is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and even more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the (B) component in the second resin composition layer, from the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion.
[0284] <(I) Other ingredients>
[0285] The first resin composition layer and the second resin composition layer may contain components other than the above-mentioned components as (I) other components as necessary.
[0286] Examples of (I) other components include resins other than the above-mentioned components, organic fillers other than (E) component, photosensitizers, polymerization inhibitors, foam stabilizers, pigments, adhesion aids such as melamine, foam stabilizers such as silicone compounds, thickeners, flame retardants, and the like.
[0287] These may be used alone or in combination of two or more.
[0288] The content of the other components (I) in the first resin composition layer or the second resin composition layer may be appropriately adjusted depending on the respective purposes, and may be 0.01 to 10 mass %, 0.05 to 5 mass %, or 0.1 to 1 mass % in the resin composition layer containing the components.
[0289] <Method for producing photosensitive multilayer resin film>
[0290] The photosensitive multilayer resin film of the present embodiment can be produced using a resin composition for forming a first resin composition layer (hereinafter also referred to as “resin composition (1)”) and a resin composition for forming a second resin composition layer (hereinafter also referred to as “resin composition (2)”).
[0291] The first resin composition layer may be formed from the resin composition (1), and the appropriate content of each component in the total solid content of the resin composition (1) is the same as the appropriate content of each component in the first resin composition layer. In addition, the second resin composition layer may be formed from the resin composition (2), and the appropriate content of each component in the total solid content of the resin composition (2) is the same as the appropriate content of each component in the second resin composition layer.
[0292] The resin composition (1) and the resin composition (2) can be produced by mixing the components to be blended in each layer and a diluent used as required. The components can be mixed using, for example, a roll mill, a bead mill, a planetary mixer, a rotation and revolution mixer, or the like.
[0293] The photosensitive multilayer resin film of the present embodiment having carrier films on both sides can be manufactured by using the resin composition (1) and the resin composition (2) to form a first resin composition layer and a second resin composition layer on respective carrier films, and then laminating the two. Alternatively, the photosensitive multilayer resin film can be manufactured by pre-forming one of the resin composition layers on a carrier film, and coating the other of the resin composition layers on the one of the resin composition layers to form the other of the resin composition layers.
[0294] Examples of the method for applying the resin composition (1) and the resin composition (2) include methods using a coating apparatus such as a notch wheel coater, a bar coater, a kiss coater, a roll coater, a gravure coater, and a die coater.
[0295] The drying temperature when drying the coating film of the resin composition (1) and the resin composition (2) is not particularly limited, but is preferably 60° C. to 150° C., more preferably 70° C. to 120° C., and even more preferably 80° C. to 100° C. The drying time is not particularly limited, but is preferably 1 minute to 60 minutes, more preferably 2 minutes to 30 minutes, and even more preferably 5 minutes to 20 minutes.
[0296] Examples of the material of the carrier film include polyesters such as polyethylene terephthalate and polybutylene terephthalate, and polyolefins such as polypropylene and polyethylene. The thickness of the carrier film is not particularly limited, but is preferably 5 μm to 100 μm, more preferably 10 μm to 60 μm, and even more preferably 15 μm to 45 μm.
[0297] [Printed wiring board and method for manufacturing the same]
[0298] The printed wiring board of the present embodiment is a printed wiring board having an interlayer insulating layer, and the interlayer insulating layer is a cured product of the photosensitive multilayer resin film of the present embodiment.
[0299] It should be noted that the “interlayer insulating layer” included in the printed wiring board of the present embodiment also includes an interlayer insulating layer in a state after various processing or treatments such as formation of through holes and wirings and roughening are performed.
[0300] The method for producing a printed wiring board according to the present embodiment is not particularly limited as long as it is a method using the photosensitive multilayer resin film according to the present embodiment, but a method for producing a printed wiring board including the following (1) to (4) is preferred.
[0301] (1): The photosensitive multilayer resin film of the present embodiment is laminated on one or both surfaces of a circuit board with the second resin composition layer being the pasting surface (hereinafter also referred to as "lamination step (1)").
[0302] (2): The photosensitive multilayer resin film laminated in the above (1) is exposed and developed to form an interlayer insulating layer having a through hole (hereinafter also referred to as "through hole forming step (2)").
[0303] (3): The interlayer insulating layer having the through-hole is heated and cured (hereinafter also referred to as "heat-curing step (3)").
[0304] (4): Forming a circuit pattern on the layer formed by curing the first resin composition layer of the interlayer insulating layer (hereinafter also referred to as "circuit pattern forming step (4)").
[0305] Below, refer to Figure 1 A method for manufacturing a printed wiring board according to the present embodiment will be described.
[0306] It should be noted that, in this specification, for convenience, a predetermined operation may be referred to as "XX step" in some cases, but this "XX step" is not limited to the method specifically described in this specification.
[0307] (Lamination process (1))
[0308] In the lamination step (1), the photosensitive multilayer resin film of the present embodiment is laminated on one or both surfaces of a circuit board in a state where the second resin composition layer is the pasting surface.
[0309] Figure 1 (a) shows a process of forming a photosensitive layer 103 on both surfaces of a substrate 101 having a circuit pattern 102 .
[0310] The photosensitive layer 103 can be formed by laminating the photosensitive multilayer resin film of this embodiment on both surfaces of the substrate 101 so that the second resin composition layer becomes the pasting surface.
[0311] The lamination may be performed by pressure bonding while applying pressure and heat using, for example, a vacuum laminator or the like.
[0312] When a carrier film is attached to the photosensitive layer 103 after lamination, the carrier film may be peeled off before exposure described later or after exposure.
[0313] (Through-hole forming step (2))
[0314] In the through-hole forming step (2), the photosensitive layer formed in the lamination step (1) is exposed and developed to form an interlayer insulating layer having a through-hole.
[0315] Figure 1 (b) shows a process of forming the interlayer insulating layer 104 having the through hole 105 by exposing and developing the photosensitive layer 103 .
[0316] By exposing the photosensitive layer 103 to light, a photoradical polymerization reaction is initiated, and the photosensitive multilayer resin film is cured.
[0317] The exposure method of the photosensitive layer 103 can be, for example, a mask exposure method in which active light is irradiated in an image form through a negative or positive mask pattern called an artwork, or a method in which active light is irradiated in an image form through a direct drawing exposure method such as an LDI (Laser Direct Imaging) exposure method or a DLP (Digital Light Processing) exposure method.
[0318] Examples of the light source for active light rays include carbon arc lamps, mercury vapor arc lamps, high pressure mercury lamps, xenon lamps, gas lasers such as argon lasers, solid lasers such as YAG lasers, and known light sources that efficiently radiate ultraviolet rays or visible light such as semiconductor lasers.
[0319] The exposure amount can be appropriately adjusted according to the light source used and the thickness of the photosensitive layer. For example, when a photosensitive layer having a thickness of 1 μm to 100 μm is exposed using ultraviolet light from a high-pressure mercury lamp, the exposure amount is not particularly limited, but is preferably 10 to 1,000 mJ / cm 2 , more preferably 50 to 700 mJ / cm 2 , more preferably 150 to 400 mJ / cm 2 .
[0320] Next, if a carrier film exists on the photosensitive layer 103, the carrier film is removed and then development is performed. In the development, the uncured portion of the photosensitive layer 103 is removed, so that the photocured portion is formed as the interlayer insulating layer 104 on the substrate.
[0321] The developing method may be wet developing or dry developing, but wet developing is preferred. As a method based on wet developing, a spray method is preferred from the viewpoint of improving resolution.
[0322] Examples of the developer include alkaline aqueous solutions, water-based developers, and organic solvent-based developers. Among these, alkaline aqueous solutions are preferred.
[0323] After exposure and development, post-exposure may be performed from the viewpoint of improving the curing degree of the interlayer insulating layer. The exposure amount in the post-exposure is not particularly limited, but is preferably 0.2 to 10 J / cm 2 , more preferably 0.5 to 5 J / cm 2 .
[0324] The shape of the through hole is not particularly limited. If described in terms of cross-sectional shape, for example, a quadrilateral, an inverted trapezoid, etc. can be listed. It should be noted that an inverted trapezoid is a shape in which the upper side is longer than the lower side. In addition, if described in terms of a top view, a circle, a quadrilateral, etc. can be listed.
[0325] In the through-hole formation by photolithography of the present embodiment, a through-hole having an inverted trapezoidal cross-sectional shape can be formed. A through-hole having such a shape is preferred because the copper plating layer has high coverage (recovery) on the through-hole wall surface.
[0326] In the through-hole formation based on the photolithography method of the present embodiment, the diameter of the through-hole can be made smaller than the diameter of the through-hole made by laser processing. The diameter of the through-hole formed by the manufacturing method of the present embodiment can be, for example, less than or equal to 40 μm, less than or equal to 35 μm, or less than or equal to 30 μm. The lower limit of the diameter of the through-hole is not particularly limited, for example, it can be greater than or equal to 15 μm, or greater than or equal to 20 μm.
[0327] (Heating and curing step (3))
[0328] In the heat curing step (3), the interlayer insulating layer having the through hole is heat cured.
[0329] That is, in the heat curing step (3), the curing reaction of the thermosetting component contained in the photosensitive multilayer resin film of the present embodiment is advanced by heating.
[0330] The heating temperature is not particularly limited, but is preferably 100 to 300° C., more preferably 120 to 200° C., and further preferably 150 to 180° C. The heating time is not particularly limited, but is preferably 0.3 to 3 hours, more preferably 0.5 to 2 hours, and further preferably 0.75 to 1.5 hours.
[0331] (Circuit pattern forming step (4))
[0332] In the interlayer insulating layer formed as described above, since the layer formed by curing the first resin composition layer is exposed, in the circuit pattern forming step (4), a circuit pattern is formed on the layer formed by curing the first resin composition layer of the interlayer insulating layer.
[0333] From the viewpoint of forming fine wiring, the circuit pattern is preferably formed by a semi-additive method in which roughening treatment, formation of a seed layer, formation of a resist pattern, formation of a copper circuit layer, and removal of the resist pattern are sequentially performed.
[0334] Roughening treatment is a treatment for roughening the surface of the interlayer insulating layer to form a concave and convex anchor point. In the case where smear occurs in the through-hole forming step (2), a roughening liquid can be used to simultaneously perform the roughening treatment and remove the smear. Examples of the roughening liquid include alkaline permanganate roughening liquids such as sodium permanganate roughening liquids; chromium / sulfuric acid roughening liquids, sodium fluoride / chromium / sulfuric acid roughening liquids, and the like.
[0335] Figure 1 (c) shows the step of forming the seed layer 106 .
[0336] The seed layer 106 is used to form a power supply layer for performing copper electroplating.
[0337] The seed layer 106 can be formed by performing chemical copper plating on the bottom of the through hole, the wall surface of the through hole, and the entire surface of the interlayer insulating layer using a palladium catalyst or the like.
[0338] Figure 1 (d) shows a step of forming a resist pattern 107 on the seed layer 106 .
[0339] The resist pattern 107 can be formed, for example, by thermally pressing a dry film resist onto the seed layer 106 using a roll laminator or the like, and then exposing and developing the resist. As the dry film resist, a commercially available product can be used.
[0340] The exposure of the dry film resist can be performed through a mask having a desired wiring pattern drawn thereon. After exposure, the dry film resist is developed using an alkaline aqueous solution to remove the unexposed portion to form a resist pattern 107. Then, a plasma treatment can be performed to remove the development residue of the dry film resist as needed.
[0341] Figure 1 (e) shows the step of forming the copper circuit layer 108.
[0342] The copper circuit layer 108 is preferably formed by copper electroplating.
[0343] As the copper electroplating solution used for copper electroplating, for example, a commercially available copper electroplating solution such as a copper electroplating solution containing copper sulfate can be used.
[0344] After copper electroplating, the resist pattern 107 is removed using an alkaline aqueous solution or an amine stripper, and then, flash etching to remove the seed layer 106 between wirings, removal of the palladium catalyst, etc. are appropriately performed by a known method. Furthermore, a post-baking treatment for sufficiently thermally curing the unreacted thermal curing component may be performed as needed.
[0345] Figure 1 (f) shows a multilayer printed wiring board 100A which is multilayered by repeating the above-mentioned steps and has a solder resist layer 109 on the outermost surface.
[0346] The solder resist layer 109 can be formed using a known photosensitive multilayer resin film for solder resist.
[0347] The above describes a method for manufacturing a printed wiring board in which a through hole is formed using the photosensitive multilayer resin film of the present embodiment, but the photosensitive multilayer resin film of the present embodiment has excellent pattern resolution, and is therefore suitable for forming a cavity for a built-in chip or passive element, for example. Regarding the cavity, for example, in the above description of the printed wiring board, the cavity can be appropriately formed by setting the drawing pattern when the photosensitive multilayer resin film is exposed to form a pattern to form a desired cavity.
[0348] [Semiconductor packaging]
[0349] The semiconductor package of the present embodiment is a semiconductor package including the printed wiring board of the present embodiment.
[0350] The semiconductor package of the present embodiment can be manufactured by, for example, mounting a semiconductor element such as a semiconductor chip or a memory on a predetermined position of a printed wiring board of the present embodiment and sealing the semiconductor element with a sealing resin or the like.
[0351] Example
[0352] Hereinafter, the present embodiment will be described in more detail with reference to Examples, but the present embodiment is not limited to these Examples.
[0353] [Measurement method of acid value]
[0354] The acid value is calculated from the amount of potassium hydroxide aqueous solution required to neutralize the measurement object.
[0355] [Method for measuring weight average molecular weight (Mw) and number average molecular weight (Mn)]
[0356] The weight average molecular weight (Mw) and number average molecular weight (Mn) were measured by the following GPC measuring device and measuring conditions, and converted and obtained using the calibration curve of standard polystyrene. In the preparation of the calibration curve, 5 sample groups ("PStQuick MP-H" and "PStQuick B", manufactured by Tosoh Corporation) were used as standard polystyrene.
[0357] (GPC measurement device)
[0358] GPC device: High-speed GPC device "HCL-8320GPC", detector is differential refractometer or UV, manufactured by Tosoh Corporation
[0359] Column: Column TSKgel SuperMultipore HZ-H (column length: 15cm, column inner diameter: 4.6mm), manufactured by Tosoh Corporation
[0360] (Measurement conditions)
[0361] Solvent: Tetrahydrofuran (THF)
[0362] Measuring temperature: 40℃
[0363] Flow rate: 0.35ml / min
[0364] Sample concentration: 10mg / THF5ml
[0365] Injection volume: 20μl
[0366] [Method for measuring weight loss by roughening treatment]
[0367] The copper foil surface of the printed wiring board substrate (Showa Denko Materials Co., Ltd., trade name "MCL-E-679") with copper foil (thickness 12 μm) laminated on the glass epoxy substrate was roughened using a roughening pretreatment liquid (MEC Co., Ltd., trade name "CZ-8100"), and then washed and dried. Next, the carrier film on the first or second resin composition layer side of the photosensitive multilayer resin film with a carrier film manufactured in each example was peeled off and removed, and the exposed first or second resin composition layer was laminated on the copper foil of the printed wiring board substrate after the roughening pretreatment in a manner that the exposed first or second resin composition layer became the adhesive surface. It should be noted that a pressing vacuum laminator (Maki Manufacturing Co., Ltd., trade name "MVLP-500") was used for lamination, and the lamination conditions were set to a pressing hot plate temperature of 70°C, a vacuuming time of 20 seconds, a lamination pressing time of 30 seconds, an air pressure of less than or equal to 4 kPa, and a crimping pressure of 0.4 MPa. After the lamination treatment, the laminate was left at room temperature for more than 1 hour to obtain an evaluation laminate in which a photosensitive multilayer resin film and a carrier film were sequentially laminated on the copper foil of the printed wiring board substrate. The laminate was irradiated with a light intensity of 400 mJ / cm using a flat exposure machine while having the carrier film of the evaluation laminate. 2 Then, the carrier film was peeled off and a high-pressure mercury lamp-type UV transport device (manufactured by ORC Manufacturing Co., Ltd.) was used to expose the film at an exposure dose of 2 J / cm 2 The layered product was irradiated with ultraviolet light at a conveying speed of 1.000 μm. Then, the layered product was heated at 170° C. for 1 hour using a hot air circulation dryer, thereby obtaining a laminated product for evaluation (1) in which the surface of the first resin composition layer was exposed and the surface of the second resin composition layer was not exposed, and a laminated product for evaluation (2) in which the surface of the second resin composition layer was exposed and the surface of the first resin composition layer was not exposed.
[0368] The evaluation laminates (1) and (2) after heating were roughened in the following manner.
[0369] The roughened laminate was immersed in a swelling solution (an aqueous solution containing Swelling DipSecuriganth P at a concentration of 49.85 mass % and sodium hydroxide at 0.3 mass %) at 70°C for 5 minutes, then immersed in an oxidizing solution (an aqueous solution containing Dosing Securiganth P500J at a concentration of 14.55 mass % and sodium hydroxide at 3.69 mass %) at 80°C for 15 minutes, and then immersed in a neutralizing solution (an aqueous solution containing Reduction Conductor Securiganth P500 at a concentration of 10.65 mass % and 95% sulfuric acid at 8.27 mass %) at 50°C for 5 minutes. Then, it was dried at 105°C for 10 minutes.
[0370] During the roughening treatment of each layer, the weight loss of the evaluation laminate (1) and the evaluation laminate (2) is calculated from the difference between the dry weight before the roughening treatment and the dry weight after the roughening treatment. The weight loss of the evaluation laminate (1) is set as the weight loss a of the first surface, and the weight loss of the evaluation laminate (2) is set as the weight loss b of the second surface, and the ratio [a / b] of the two is calculated.
[0371] [Manufacturing of photosensitive multilayer resin film]
[0372] Examples 1 to 7, Comparative Examples 1 to 2
[0373] The components were mixed according to the composition shown in Table 1 (the unit of the numerical values in the table is parts by mass, and in the case of a solution, it is the amount converted to solid content), and kneaded using a three-roll mill and a rotation and revolution mixer. Thereafter, methyl ethyl ketone was added so that the solid content concentration became 65% by mass, and a resin composition (1) for forming a first resin composition layer and a resin composition (2) for forming a second resin composition layer were obtained.
[0374] Next, the resin composition (1) was coated on a carrier film (PET film, manufactured by Teijin Limited, trade name "G2-16", thickness 16 μm) and dried at 100° C. for 10 minutes using a hot air convection dryer to form a first resin composition layer with a carrier film (the thickness of the first resin composition layer was 5 μm).
[0375] In addition, the resin composition (2) was coated on a carrier film different from the above (PET film manufactured by Teijin Limited, trade name "G2-16", thickness 16 μm), and dried at 100°C for 10 minutes using a hot air convection dryer to form a second resin composition layer with a carrier film (the thickness of the second resin composition layer was 20 μm).
[0376] By bonding the above-obtained first resin composition layer with a carrier film and the second resin composition layer with a carrier film to each other, a photosensitive multilayer resin film with a carrier film (the thickness of the photosensitive multilayer resin film is 25 μm) is obtained, which has a carrier film, a first resin composition layer, a second resin composition layer and a carrier film in sequence.
[0377] The following evaluations were performed using the produced photosensitive multilayer resin film.
[0378] [Determination of relative dielectric constant (Dk) and dielectric loss tangent (Df)]
[0379] Two films were prepared in which the carrier film on the second resin composition layer side of the photosensitive multilayer resin film with a carrier film produced in each example was peeled off and removed, and the second resin composition layers were bonded to each other.
[0380] Next, with the carrier films on both sides, the substrate was irradiated with a light intensity of 400 mJ / cm using a flat exposure machine. 2 Then, the carrier films on both sides were peeled off and the UV exposure machine was used to irradiate the film at a light intensity of 2 J / cm 2 Then, the sample was heated at 170°C for 1 hour using a hot air circulation dryer and cut into pieces of 7 cm x 10 cm in size to prepare a sample for measuring relative dielectric constant (Dk) and dielectric loss tangent (Df).
[0381] The obtained measurement sample was dried at 105°C for 10 minutes using a hot air circulation dryer, and then the relative dielectric constant (Dk) and dielectric loss tangent (Df) were measured in the 10 GHz frequency band using a separated column dielectric resonator method (SPDR method), and evaluated according to the following criteria.
[0382] (Evaluation criteria for relative dielectric constant (Dk))
[0383] A: Less than or equal to 2.8
[0384] B: greater than 2.8 to less than or equal to 3.0
[0385] C: greater than 3.0
[0386] (Evaluation criteria for dielectric loss tangent (Df))
[0387] A: Less than or equal to 0.0100
[0388] B: greater than 0.0100 to less than or equal to 0.0120
[0389] C: greater than 0.0120
[0390] [Evaluation of through-hole resolution]
[0391] (1) Preparation of evaluation laminate
[0392] The copper foil surface of the printed wiring board substrate (Showa Denko Materials Co., Ltd., trade name "MCL-E-679") with copper foil (thickness 12 μm) laminated on the glass epoxy substrate was roughened using a roughening pretreatment liquid (MEC Co., Ltd., trade name "CZ-8100"), and then washed and dried. Next, the carrier film on the second resin composition layer side of the photosensitive multilayer resin film with a carrier film manufactured in each example was peeled off and removed, and the exposed second resin composition layer was laminated on the copper foil of the printed wiring board substrate after the roughening pretreatment in a manner that the exposed second resin composition layer became the adhesive surface. It should be noted that a pressing vacuum laminator (Maki Manufacturing Co., Ltd., trade name "MVLP-500") was used for lamination, and the lamination conditions were set to a pressing hot plate temperature of 70°C, a vacuuming time of 20 seconds, a lamination pressing time of 30 seconds, an air pressure of less than or equal to 4 kPa, and a crimping pressure of 0.4 MPa. After the lamination treatment, the film was left to stand at room temperature for 1 hour or more, thereby obtaining a laminate for evaluation in which a photosensitive multilayer resin film and a carrier film were laminated in this order on the copper foil surface of the printed wiring board substrate.
[0393] (2) Sensitivity measurement
[0394] A 41-step exposure meter was placed on the carrier film on the first resin composition layer side of the evaluation laminate obtained above. Next, exposure was performed using a direct imaging exposure device (manufactured by ORC Manufacturing Co., Ltd., trade name "DXP-3512") using an ultra-high pressure mercury lamp as a light source. The exposure pattern used was The points are arranged in a grid-like dot pattern.
[0395] After exposure, the film was left at room temperature for 30 minutes, and then the carrier film on the first resin composition layer side of the evaluation laminate obtained above was removed. The photosensitive multilayer resin film in the unexposed part was spray-developed for 60 seconds using a 1 mass % sodium carbonate aqueous solution at 30°C. After development, the exposure energy when the gloss residual stage number of the 41-stage step exposure meter reached 4.0 was taken as the sensitivity of the photosensitive multilayer resin film (unit: mJ / cm 2 ). Using the pattern exposed at this sensitivity, evaluation was performed according to the following evaluation criteria.
[0396] (3) Evaluation of through-hole resolution
[0397] The resolution of the through-holes was evaluated by observing a through-hole pattern formed by exposure and spray development at the sensitivity, ie, exposure energy, of the photosensitive multilayer resin film determined in (2) above using an optical microscope and evaluating the resolution based on the following criteria.
[0398] (Evaluation Criteria)
[0399] A: Dot pattern The through hole is partially open.
[0400] C: Dot pattern The through hole portion is not opened.
[0401] [Evaluation of bonding strength with copper plating]
[0402] (1) Preparation of evaluation laminate and measurement of sensitivity of photosensitive multilayer resin film
[0403] In the steps (1) and (2) of the above-mentioned [Evaluation of the resolution of through holes], except that the exposure machine used was changed to a parallel light exposure machine using an ultra-high pressure mercury lamp as a light source (manufactured by ORC Manufacturing Co., Ltd., trade name "EXM-1201"), the same operation as in the steps (1) and (2) of the above-mentioned [Evaluation of the resolution of through holes] was performed to prepare a laminate for evaluation, and the exposure energy when the gloss residual stage number was 8.0 was calculated and used as the sensitivity (unit: mJ / cm 2 ).
[0404] (2) Exposure and Development Process
[0405] The carrier film on the first resin composition layer side of the evaluation laminate was peeled off and the entire surface was exposed at the sensitivity, i.e., exposure energy, obtained above, to cure the photosensitive multilayer resin film. After exposure, the film was left at room temperature for 30 minutes, and then the unexposed portion of the photosensitive multilayer resin film was spray developed for 60 seconds using a 1 mass % sodium carbonate aqueous solution at 30°C.
[0406] (3) Post-curing treatment
[0407] Next, a high-pressure mercury lamp irradiation type UV delivery device (manufactured by ORC Manufacturing Co., Ltd.) was used to expose the sample at an exposure dose of 2 J / cm 2 The film was then post-cured with UV light at a conveying speed of 1.50°C. Then, it was heated at 170°C for 1 hour using a hot air circulation dryer.
[0408] (4) Roughening treatment
[0409] The heated evaluation laminate was treated with a swelling liquid "Swelling Dip Securiganth P" at 70°C for 5 minutes, and then roughened with a roughening liquid "Dosing Securiganth P500J" at 70°C for 10 minutes. Next, a neutralization treatment was performed at 50°C for 5 minutes using a neutralizing liquid "Reduction Conduction Securiganth P500". Then, a hydrofluoric acid treatment was performed at room temperature for 10 minutes using a buffered hydrofluoric acid "LAL1800 SA High Purity Buffered Hydrofluoric Acid". It should be noted that the swelling liquid, the roughening liquid, and the neutralizing liquid were all made by ATOTECH JAPAN Co., Ltd., and the buffered hydrofluoric acid was made by Stella Chemifa Co., Ltd.
[0410] (5) Plating treatment
[0411] The roughened laminate was subjected to chemical plating at 30°C for 15 minutes using a chemical plating solution "Priganth MSK-DK" (manufactured by ATOTECH JAPAN Co., Ltd.). Then, the roughened laminate was subjected to chemical plating at 24°C, 2 A / dm 2 The electroplating treatment was performed for 1.5 hours to form copper plating on the interlayer insulating layer. The thickness of the copper plating was 25 μm.
[0412] (6) Determination of bonding strength with copper plating
[0413] The adhesive strength with the copper plating layer was measured by vertical peeling strength at 23° C. in accordance with JIS C6481:1996 and evaluated according to the following criteria.
[0414] (Evaluation Criteria)
[0415] A: greater than 0.4kN / m
[0416] B: greater than 0.1kN / m to less than or equal to 0.4kN / m
[0417] C: less than or equal to 0.1kN / m
[0418] [Table 1]
[0419] Table 1
[0420]
[0421] The details of each component described in Table 1 are as follows.
[0422] [(A) ingredient]
[0423] Compound having a carboxyl group and an acryloyl group: manufactured by Nippon Kayaku Co., Ltd., trade name "ZXR-1807H", acid value: 110 mgKOH / g, weight average molecular weight (Mw): 2,000
[0424] [(B) ingredient]
[0425] · Biphenyl aralkyl type epoxy resin: manufactured by Nippon Kayaku Co., Ltd., trade name "NC-3000-L", epoxy equivalent: 272 g / eq
[0426] · Naphthol-type epoxy resin: manufactured by Nippon Steel & Sumitomo Metal Corporation, trade name "ESN-475V", epoxy equivalent: 325 g / eq
[0427] Maleimide resin: Aromatic bismaleimide resin with indane skeleton
[0428] ·Allyl resin: diallyl isocyanurate compound, manufactured by Shikoku Chemical Industry Co., Ltd., trade name "LDAIC"
[0429] [(C) ingredient]
[0430] Photopolymerization initiator 1: phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide
[0431] Photopolymerization initiator 2: 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyl oxime)
[0432] [(D) ingredient]
[0433] Silica 1: manufactured by Admatechs Co., Ltd., trade name "SC2050-MB", average particle size (D 50 ): 0.5μm, true density 2,200kg / m 3
[0434] Silica 2: manufactured by TAT, trade name "BQQ-0710SCB", average particle size (D 50 ): 0.7μm, true density 1,350kg / m 3
[0435] [(E) ingredient]
[0436] Polytetrafluoroethylene particles: manufactured by Mitsubishi Pencil Co., Ltd., trade name "MPT-N8", average particle size (D 50 ): 0.2~0.3μm
[0437] [(F)INGREDIENT]
[0438] Polybutadiene-based elastomer: butadiene-styrene-random copolymer, manufactured by Cray Valley, trade name "Ricon 100", number average molecular weight (Mn): 4,500
[0439] · Acid anhydride-modified polybutadiene: manufactured by Cray Valley Corporation, trade name “Ricon 131 MA17”, number average molecular weight (Mn): 5,400, number of acid anhydride groups in one molecule: 9
[0440] [(G) ingredient]
[0441] Organic peroxide: 1,3-di(tert-butylperoxyisopropyl)benzene
[0442] [(H) ingredient]
[0443] Curing accelerator: 1-benzyl-2-phenylimidazole
[0444] [(I)INGREDIENTS]
[0445] Sensitizer: 4,4'-bis-(diethylamino)benzophenone
[0446] ·Inhibitor: 4-tert-butylcatechol
[0447] As can be seen from Table 1, the cured products formed from the photosensitive multilayer resin films of Examples 1 to 7 of the present embodiment all have excellent dielectric properties and high conductor adhesion.
[0448] Description of Reference Numerals
[0449] 100A: Multilayer printed wiring board
[0450] 101: Substrate
[0451] 102: Circuit pattern
[0452] 103: Photosensitive layer
[0453] 104: Interlayer insulation layer
[0454] 105: Through hole
[0455] 106: Seed layer
[0456] 107: Resist pattern
[0457] 108: Copper circuit layer
[0458] 109: Solder mask layer.
Claims
1. A photosensitive multilayer resin film comprising a first resin composition layer and a second resin composition layer, The first resin composition layer and the second resin composition layer respectively contain: (A) a compound having an ethylenically unsaturated group, (B) a thermosetting resin, (C) a photopolymerization initiator, and (D) an inorganic filler. The photosensitive multilayer resin film is irradiated with 2 J / cm 2 After being exposed to ultraviolet rays, it was heated at 170°C for 1 hour to cure, and then, The weight loss when the roughening treatment is performed under the following roughening treatment conditions in a state where the surface of the first resin composition layer is exposed and the surface of the second resin composition layer is not exposed is defined as a, When the weight loss amount when the roughening treatment is performed under the following roughening treatment conditions in a state where the surface of the second resin composition layer is exposed and the surface of the first resin composition layer is not exposed is defined as b, a is less than b, and a is less than or equal to 10g / m 2 , Roughening conditions: The roughened object was immersed in a swelling solution at 70° C. for 5 minutes, then immersed in an oxidizing agent solution at 80° C. for 15 minutes, and further immersed in a neutralizing solution at 50° C. for 5 minutes, and then dried. 2 . The photosensitive multilayer resin film according to claim 1 , wherein each of the first resin composition layer and the second resin composition layer contains a compound having an ethylenically unsaturated group and an acidic substituent as the (A) compound having an ethylenically unsaturated group. 3 . The photosensitive multilayer resin film according to claim 1 , wherein the first resin composition layer and the second resin composition layer each contain at least one selected from the group consisting of epoxy resins, maleimide resins, allyl resins and vinyl resins as the (B) thermosetting resin.
4. According to the photosensitive multilayer resin film according to claim 3, the first resin composition layer and the second resin composition layer respectively contain epoxy resin as the (B) thermosetting resin, and the content of the epoxy resin in the first resin composition layer calculated on a mass basis is greater than the content of the epoxy resin in the second resin composition layer calculated on a mass basis. 5 . The photosensitive multilayer resin film according to claim 1 , wherein the first resin composition layer contains silicon dioxide as the (D) inorganic filler, and a content of the silicon dioxide in the first resin composition layer is 5 to 70% by mass.
6. The photosensitive multilayer resin film according to claim 1, wherein the second resin composition layer contains a3 Silica is used as (D) inorganic filler.
7. The photosensitive multilayer resin film according to claim 1, wherein the second resin composition layer further contains (E) a fluorine-containing resin, and the content of the (E) fluorine-containing resin is 10 to 70% by mass based on the total amount of resin components in the second resin composition layer. 8 . The photosensitive multilayer resin film according to claim 1 , wherein each of the first resin composition layer and the second resin composition layer further contains (F) an elastomer. 9 . The photosensitive multilayer resin film according to claim 1 , wherein a content of the inorganic filler (D) in the second resin composition layer is less than 60% by mass.
10. The photosensitive multilayer resin film according to claim 1, wherein the layer formed by curing the first resin composition layer is a layer having a circuit pattern formed by copper plating, and the second resin composition layer is a layer having a surface to be attached when laminating the photosensitive multilayer resin films. 11 . The photosensitive multilayer resin film according to claim 1 , which is used to form an interlayer insulating layer having an optical through hole. 12 . A printed wiring board comprising an interlayer insulating layer which is a cured product of the photosensitive multilayer resin film according to claim 1 .
13. A semiconductor package comprising the printed wiring board according to claim 12.
14. A method for manufacturing a printed wiring board, comprising the following (1) to (4): (1) The photosensitive multilayer resin film according to any one of claims 1 to 11 is laminated on one or both sides of a circuit substrate in a state where the second resin composition layer becomes an adhesive surface; (2): exposing and developing the photosensitive multilayer resin film laminated in (1) to form an interlayer insulating layer having a through hole; (3): heating and curing the interlayer insulating layer having the through hole; as well as (4): A circuit pattern is formed on the layer formed by curing the first resin composition layer of the interlayer insulating layer.
Citation Information
Patent Citations
Photosensitive resin composition, and dry film, printed wiring board and method for manufacturing printed wiring board using the composition
JP2017116652A