Hydrogel wet chamber glasses for xerophthalmia as well as preparation method and application of hydrogel wet chamber glasses

Through hydrogel wet room mirrors with polyvinyl alcohol, sodium polyacrylate and nanocellulose materials, the existing wet room mirror water storage tank is solved, and the high water content and long-term moisturizing effect is achieved. Suitable for dry eye treatment.

CN119015043APending Publication Date: 2024-11-26CHENGDU SHICHUANG TECHNOLOGY MATERIALS MEDICAL EQUIPMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411136457.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

When treating dry eye disease, the existing wet room mirrors have problems such as small water storage tank size, frequent addition of fluids, and large weight of the rear lens after increasing the equipment, which is not suitable for long-term wear.

Method used

The hydrogel wet chamber mirror is prepared using polyvinyl alcohol, sodium polyacrylate and nanocellulose. Through surface activation modification and freeze-thawing cycle, a hydrogel moisturizing coating with high water content, transparent and adhesion is formed. layer.

Benefits of technology

It realizes the excellent moisturizing properties and biocompatibility of hydrogel wet room mirrors, which are suitable for long-term wear, reducing the defects of frequent liquid addition and the volume and weight of the lens.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119015043A_ABST
    Figure CN119015043A_ABST
Patent Text Reader

Abstract

The invention discloses hydrogel wet chamber glasses for xerophthalmia and a preparation method and application thereof, and relates to the field of medical products, the method comprises the following steps: dissolving polyvinyl alcohol in water at 95 DEG C to form a solution A; dissolving sodium polyacrylate in water to form a solution B; dispersing nanocellulose in water to form a suspension C; dissolving trihydroxymethyl aminomethane in water, and adjusting the pH value to form a solution D; dissolving dopamine in the solution D to obtain a solution E; soaking the spectacle frame in the solution E, performing surface activation modification, washing and drying treatment, and collecting the modified spectacle frame; soaking the modified glasses frame in a mixed solution of the solution A, the solution B and the suspension C, performing multiple times of freezing and unfreezing circulation treatment, and collecting the glasses frame loaded with the hydrogel moisturizing coating to obtain the hydrogel wet chamber glasses for xerophthalmia.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of medical products, and in particular to a hydrogel wet chamber lens for dry eye and a preparation method and application thereof. Background Art

[0002] Refractive surgery, double eyelid surgery, etc. will cause certain damage to the eyes, which takes a while to heal. At this time, the eyelids are in a stalemate state, and dry eyes will occur, including dryness after eye surgery. Dry eyes refer to abnormal tear quality or quantity or abnormal dynamics caused by any reason, which leads to decreased tear film stability, accompanied by eye discomfort and ocular surface tissue lesions. The current treatment methods for patients with dry eyes can be roughly divided into the following categories: 1. Use relevant eye drops for hydration and drug treatment. 2. Wear goggles with a sealed effect to lock in the moisture evaporated by the eyeball itself in a closed environment. 3. Wear goggles with moisturizing accessories.

[0003] However, using eye drops for moisturizing has the following disadvantages: 1) It cannot achieve the effect of long-term moisturizing; 2) Most eye drops contain preservatives, which may damage the eyes if used for a long time; 3) Long-term use of eye drops will produce drug resistance and reduce the function of eye drops. However, existing wet room glasses have the following defects: 1) Since the water storage tank is installed in the grooves on the left and right outer sides of the frame, it is necessary to provide liquid medicine through two water storage tanks respectively, so as to achieve atomization and humidification of the eyes on both sides. The two water storage tanks not only have multiple operations of adding liquid and disassembly and assembly, but also inevitably increase the disassembly and assembly structure of the water storage tank and the frame, which is not conducive to reducing production costs; 2) Since the water storage tank is embedded in the groove on the frame, the volume of the water storage tank cannot be too large, resulting in a small capacity, which is not conducive to long-term wear and use by users and requires repeated filling of liquid. 3) After adding the atomization device, the volume and weight of the glasses are increased, which is not suitable for long-term wear. Summary of the invention

[0004] In order to solve the above-mentioned technical problems existing in the prior art, the present application provides a hydrogel wet chamber lens for dry eye and its preparation method and application, so as to solve the problem that myopia cannot be solved by wearing special dry eye glasses when suffering from myopia or dry eye after surgery mentioned in the above-mentioned background technology.

[0005] In order to achieve the above purpose, the technical solution of the embodiment of the present application is:

[0006] The first aspect of the present application provides a method for preparing a hydrogel wet chamber lens for dry eye, comprising the following steps:

[0007] Dissolve polyvinyl alcohol in 95°C water to form solution A; dissolve sodium polyacrylate in water to form solution B; disperse nanocellulose in water to form suspension C; dissolve tris(hydroxymethyl)aminomethane in water and adjust the pH to form solution D; dissolve dopamine in solution D to obtain solution E;

[0008] Immersing the frame in the solution E, performing surface activation modification, washing, and drying, and collecting the modified frame;

[0009] The modified frame is immersed in a mixed solution of the solution A, the solution B and the suspension C, and subjected to multiple freeze-thaw cycles, and the frame with the hydrogel moisturizing coating is collected to obtain a hydrogel wet chamber lens for dry eye.

[0010] In combination with the first aspect, preferably, the content of polyvinyl alcohol in the solution A is 15wt%;

[0011] And / or, the concentration of sodium polyacrylate in the solution B is 15wt%;

[0012] and / or, the concentration of nanocellulose in the solution C is 15 wt %;

[0013] And / or, the concentration of tris(hydroxymethyl)aminomethane in the solution D is 10 mmol / L;

[0014] And / or, the concentration of dopamine in the solution E is 2 mg / mL.

[0015] In combination with the first aspect, preferably, the pH value of the solution D is 7.5-8.5.

[0016] In combination with the first aspect, preferably, the thickness of the hydrogel moisturizing coating is 3 to 4 mm.

[0017] In combination with the first aspect, preferably, the polyvinyl alcohol is type 1797 polyvinyl alcohol.

[0018] In combination with the first aspect, preferably, when the polyvinyl alcohol is dissolved in 95° C. water, the dissolution time is 2 hours;

[0019] And / or, when the sodium polyacrylate is dissolved in water, the dissolution time is 2 hours;

[0020] And / or, the nanocellulose is dispersed in water for 2 hours.

[0021] In combination with the first aspect, preferably, when the modified base plate is immersed in the mixed solution of the solution A, the solution B and the suspension C, the immersion temperature is 27° C. and the immersion time is 24 hours.

[0022] In combination with the first aspect, preferably, when the multiple freezing cycles are performed, the freezing time is 8 hours;

[0023] And / or, when the hydrogel moisturizing coating is thawed, the thawing time is 4 hours.

[0024] The second aspect of the present application provides a hydrogel wet chamber lens for dry eye as described in the first aspect.

[0025] The third aspect of the present application provides a use of a hydrogel wet chamber lens for dry eye prepared by the method described in the first aspect or a hydrogel wet chamber lens for dry eye described in the second aspect in the treatment of dry eye.

[0026] Compared with the prior art, the advantages or beneficial effects of the embodiments of the present application include at least:

[0027] The preparation method provided in the present application activates the surface of the frame after surface modification, enables polymer grafting on the surface of the frame, and improves the adhesion performance of the hydrogel material on the smooth frame; at the same time, the photocured cross-linked hydrogel exhibits good transparency and excellent adhesion, high water content and biocompatibility, which indicates that the hydrogel wet chamber lens used for dry eye has excellent moisturizing properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a schematic diagram of the structure of the hydrogel wet room mirror prepared in Example 7;

[0029] Figure 2 This is a photo of the polyvinyl alcohol hydrogel prepared in Example 7 adhered to PMMA;

[0030] Figure 3 This is a photo of the polyvinyl alcohol hydrogel prepared in Example 20 adhered to ABS;

[0031] Figure 4 The water loss rate of the polyvinyl alcohol hydrogel wet chamber mirror prepared in Example 7 in an open environment;

[0032] Figure 5 The water loss rate of the polyvinyl alcohol hydrogel wet room mirror prepared in Example 7 in a closed environment;

[0033] Figure 6 This is the moisture retention rate of the polyvinyl alcohol hydrogel wet room mirror prepared in Example 7 in a closed environment.

[0034] Figure ID

[0035] Lens 1, hydrogel coating 2. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings. The described embodiments should not be regarded as limiting the present application. All other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of this application.

[0037] In the following description, reference is made to "some embodiments", which describe a subset of all possible embodiments, but it is understood that "some embodiments" may be the same subset or different subsets of all possible embodiments, and may be combined with each other without conflict. Unless otherwise defined, all technical and scientific terms used in the embodiments of the present application have the same meaning as those commonly understood by those skilled in the art of the technical field of the embodiments of the present application. The terms used in the embodiments of the present application are only for the purpose of describing the embodiments of the present application and are not intended to limit the present application.

[0038] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.

[0039] It should be noted that all raw materials / reagents in the examples of the present application can be purchased on the market or prepared according to conventional methods well known to those skilled in the art; the term "and / or" in the examples of the present application is only used to describe the association relationship between associated objects, indicating that three relationships may exist, for example, A and / or B means the existence of A alone, B alone, and A and B at the same time, among which A and B can be singular or plural, and the character " / " generally indicates that the associated objects before and after are in an "or" relationship.

[0040] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0041] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0042] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0043] Those skilled in the art will appreciate that the numerical ranges in the examples of the present application are to be understood as specifically disclosing each intermediate value between the upper and lower limits of the range. Each smaller range between the intermediate values ​​in any stated value and stated range and any other stated value or intermediate value in the range is also included in the present application. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.

[0044] Unless otherwise stated, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art in the field described in the present application. Although the present application only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the embodiments or test cases of the present application. All documents mentioned in this specification are generally incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of the present application shall prevail.

[0045] It should be noted that all raw materials and / or reagents in the examples of the present application are purchased on the market or prepared according to conventional methods well known to those skilled in the art.

[0046] In a first aspect, the present invention provides a method for preparing a hydrogel wet chamber lens for dry eye, comprising the following steps:

[0047] Dissolve polyvinyl alcohol in 95°C water to form solution A; dissolve sodium polyacrylate in water to form solution B; disperse nanocellulose in water to form suspension C; dissolve tris(hydroxymethyl)aminomethane in water and adjust the pH to form solution D; dissolve dopamine in solution D to obtain solution E;

[0048] Immersing the frame in the solution E, performing surface activation modification, washing, and drying, and collecting the modified frame;

[0049] The modified frame is immersed in a mixed solution of the solution A, the solution B and the suspension C, and subjected to multiple freeze-thaw cycles, and the frame with the hydrogel moisturizing coating is collected to obtain a hydrogel wet chamber lens for dry eye.

[0050] The preparation method provided in the present application activates the surface of the frame after surface modification, enables polymer grafting on the surface of the frame, and improves the adhesion performance of the hydrogel material on the smooth frame; at the same time, the photocured cross-linked hydrogel exhibits good transparency and excellent adhesion, high water content and biocompatibility, which indicates that the hydrogel wet chamber lens used for dry eye has excellent moisturizing properties.

[0051] In a specific embodiment, the content of polyvinyl alcohol in solution A of the embodiment of the present application is preferably 15 wt %.

[0052] In a specific embodiment, the content of sodium polyacrylate in solution B of the embodiment of the present application is preferably 15 wt %.

[0053] In a specific embodiment, the content of nanocellulose in solution C of the embodiment of the present application is preferably 15 wt %.

[0054] In a specific embodiment, the concentration of tris(hydroxymethyl)aminomethane in solution D of the embodiment of the present application is preferably 10 mmol / L.

[0055] In a specific embodiment, the concentration of dopamine in solution E of the present embodiment is preferably 2 mg / mL.

[0056] In a specific embodiment, the pH value of solution D in the embodiment of the present application is preferably 7.5 to 8.5.

[0057] In a specific embodiment, the thickness of the hydrogel moisturizing coating of the embodiment of the present application is preferably 3 to 4 mm.

[0058] In a specific embodiment, the polyvinyl alcohol in the embodiment of the present application is preferably type 1797 polyvinyl alcohol.

[0059] In a specific embodiment, when polyvinyl alcohol is dissolved in 95° C. water in the embodiment of the present application, the dissolution time is preferably 2 hours.

[0060] In a specific embodiment, when sodium polyacrylate is dissolved in water in the embodiment of the present application, the dissolution time is preferably 2 hours.

[0061] In a specific embodiment, the nanocellulose is dispersed in water in the present application, and the dispersion time is preferably 2 hours.

[0062] In a specific embodiment, when the modified base plate material of the embodiment of the present application is immersed in a mixed solution of solution A, solution B and suspension C, the immersion temperature is preferably 27° C., and the immersion time is preferably 24 hours.

[0063] In a specific embodiment, when multiple freezing cycles are performed in the embodiment of the present application, the freezing time is preferably 8 hours.

[0064] In a specific embodiment, when the hydrogel moisturizing coating is thawed in the embodiment of the present application, the thawing time is preferably 4 hours.

[0065] In a second aspect, an embodiment of the present application provides a hydrogel wet chamber lens for dry eye prepared by the method described in the first aspect.

[0066] In a third aspect, an embodiment of the present application provides a use of a hydrogel wet chamber lens for dry eye prepared by the method described in the first aspect or a hydrogel wet chamber lens for dry eye described in the second aspect in the treatment of dry eye.

[0067] The technical method of the present application will be further described below in conjunction with specific embodiments.

[0068] Example 1

[0069] This embodiment 1 provides a method for preparing a hydrogel wet chamber lens 1 for dry eye, and the specific steps are as follows:

[0070] Dissolve polyvinyl alcohol in 95°C water to form solution A; dissolve sodium polyacrylate in water to form solution B; disperse nanocellulose in water to form suspension C; dissolve tris(hydroxymethyl)aminomethane in water and adjust the pH to form solution D; dissolve dopamine in solution D to obtain solution E;

[0071] Immersing the frame in the solution E, performing surface activation modification, washing, and drying, and collecting the modified frame;

[0072] The modified frame is immersed in a mixed solution of the solution A, the solution B and the suspension C, and subjected to multiple freeze-thaw cycles, and the frame with the hydrogel moisturizing coating is collected to obtain a hydrogel wet chamber lens 1 for dry eye.

[0073] The ratio of solution A, solution B and suspension C is 1:0:0, and the base plate is a polymethyl methacrylate (PMMA) frame.

[0074] Example 2

[0075] A hydrogel wet chamber lens 2 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 0:1:0, and the base plate was a polymethyl methacrylate (PMMA) lens frame.

[0076] Example 3

[0077] A hydrogel wet chamber lens 3 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 0:0:1, and the base plate material was a polymethyl methacrylate (PMMA) lens frame.

[0078] Example 4

[0079] A hydrogel wet chamber lens 4 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:1:0, and the base plate material was a polymethyl methacrylate (PMMA) lens frame.

[0080] Example 5

[0081] A hydrogel wet chamber lens 5 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:0:1, and the base plate material was a polymethyl methacrylate (PMMA) lens frame.

[0082] Example 6

[0083] A hydrogel wet chamber lens 6 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 0:1:1, and the base plate material was polymethyl methacrylate (PMMA) lens frame.

[0084] Example 7

[0085] A hydrogel wet chamber lens 7 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:1:1, and the base plate material was a polymethyl methacrylate (PMMA) lens frame.

[0086] Example 8

[0087] A hydrogel wet chamber lens 8 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:1:2, and the base plate material was a polymethyl methacrylate (PMMA) lens frame.

[0088] Example 9

[0089] A hydrogel wet chamber lens 9 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:2:1, and the base plate material was a polymethyl methacrylate (PMMA) lens frame.

[0090] Example 10

[0091] A hydrogel wet chamber lens 10 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 2:1:1, and the base plate material was a polymethyl methacrylate (PMMA) lens frame.

[0092] Embodiment 11

[0093] A hydrogel wet chamber lens 11 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 2:2:1, and the base plate material was a polymethyl methacrylate (PMMA) lens frame.

[0094] Example 12

[0095] A hydrogel wet chamber lens 12 for dry eye is prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C is 2:1:2, and the base plate is a polymethyl methacrylate PMMA lens frame.

[0096] Embodiment 13

[0097] A hydrogel wet chamber lens 13 for dry eye is prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C is 1:2:2, and the base plate is a polymethyl methacrylate PMMA lens frame.

[0098] Embodiment 14

[0099] A hydrogel wet chamber lens 14 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:0:0, and the base plate material was an ABS plastic frame.

[0100] Embodiment 15

[0101] A hydrogel wet chamber lens 2 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 0:1:0, and the base plate material was an ABS plastic frame.

[0102] Example 16

[0103] A hydrogel wet chamber lens 3 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 0:0:1, and the base plate material was an ABS plastic frame.

[0104] Embodiment 17

[0105] A hydrogel wet chamber lens 4 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:1:0, and the base plate material was an ABS plastic frame.

[0106] Embodiment 18

[0107] A hydrogel wet chamber lens 5 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:0:1, and the base plate material was an ABS plastic frame.

[0108] Embodiment 19

[0109] A hydrogel wet chamber lens 6 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 0:1:1, and the base plate material was an ABS plastic frame.

[0110] Embodiment 20

[0111] A hydrogel wet chamber lens 7 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:1:1, and the base plate material was an ABS plastic frame.

[0112] Embodiment 21

[0113] A hydrogel wet chamber lens 8 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:1:2, and the base plate material was an ABS plastic frame.

[0114] Embodiment 22

[0115] A hydrogel wet chamber lens 9 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:2:1, and the base plate material was an ABS plastic lens frame.

[0116] Embodiment 23

[0117] A hydrogel wet chamber lens 10 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 2:1:1, and the base plate material was an ABS plastic frame.

[0118] Embodiment 24

[0119] A hydrogel wet chamber lens 11 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 2:2:1, and the base plate was ABS plastic.

[0120] Embodiment 25

[0121] A hydrogel wet chamber lens 12 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 2:1:2, and the base plate material was an ABS plastic frame.

[0122] Embodiment 26

[0123] A hydrogel wet chamber lens 13 for dry eye was prepared according to the method of Example 1, except that the ratio of solution A, solution B and suspension C was 1:2:2, and the base plate material was an ABS plastic lens frame.

[0124] In order to verify the relevant performance of the hydrogel wet chamber lens 1-26 for dry eye prepared in Examples 1-26, data tests were performed on the prepared hydrogel wet chamber lens 1-26 for dry eye. The test results are shown in Tables 1 to 6. Table 1 shows the water loss rate of the hydrogel wet chamber lens for dry eye prepared in Examples 1-26 exposed to a room temperature humid environment (25°C, humidity 60%); Table 2 shows the water loss rate of the hydrogel wet chamber lens for dry eye prepared in Examples 1-26 exposed to a room temperature dry environment (25°C, humidity 20%); Table 3 shows the water loss rate of the hydrogel wet chamber lens for dry eye prepared in Examples 1-26 exposed to a body temperature environment (37°C); Table 4 shows the water loss rate of the hydrogel wet chamber lens for dry eye prepared in Examples 1-26 sealed at room temperature (25°C); Table 5 shows the water loss rate of the hydrogel wet chamber lens for dry eye prepared in Examples 1-26 The water loss rate of the prepared hydrogel wet chamber mirror for dry eye 1-26 sealed in a room temperature dry environment (25°C, humidity 20%); Table 6 is the water loss rate of the hydrogel wet chamber mirror for dry eye prepared in Examples 1-26 sealed in a body temperature environment (37°C); Table 7 is the water loss rate of the hydrogel wet chamber mirror for dry eye prepared in Examples 1-26 sealed in a room temperature humid environment (25°C, humidity 60%); Table 7 is the moisture retention rate of the hydrogel wet chamber mirror for dry eye prepared in Examples 1-26 sealed in a room temperature environment (25°C); Table 8 is the moisture retention rate of the hydrogel wet chamber mirror for dry eye prepared in Examples 1-26 sealed in a dry environment (25°C, temperature 20%); Table 9 is the moisture retention rate of the hydrogel wet chamber mirror for dry eye prepared in Examples 1-26 sealed in a body temperature environment (37°C).

[0125] Table 1 Water loss rate of the hydrogel wet room lens for dry eye prepared in Examples 1-26 exposed to a room temperature humid environment (25°C, humidity 60%)

[0126]

[0127] Table 2 Water loss rate of the hydrogel wet room lens for dry eye prepared in Examples 1-26 exposed to a dry environment at room temperature (25°C, humidity 20%)

[0128]

[0129]

[0130] Table 3 Water loss rate of the hydrogel wet chamber lens for dry eye prepared in Examples 1-26 exposed to body temperature environment (37°C)

[0131]

[0132]

[0133] Table 4 Water loss rate of hydrogel wet-room lenses for dry eye prepared in Examples 1-26 sealed at room temperature (25°C)

[0134]

[0135] Table 5 Water loss rate of the hydrogel wet-room lenses for dry eye prepared in Examples 1-26 sealed in a dry environment (25°C, humidity 20%)

[0136]

[0137]

[0138] Table 6 Water loss rate of hydrogel wet chamber lenses for dry eye prepared in Examples 1-26 sealed in a body temperature environment (37°C)

[0139]

[0140] Table 7 Moisture retention rate of the hydrogel wet room lens for dry eye prepared in Examples 1-26 sealed in room temperature environment (25°C)

[0141]

[0142] Table 8 Moisture retention rate of the hydrogel wet-room lenses for dry eye prepared in Examples 1-26 sealed in a dry environment (25°C, temperature 20%)

[0143]

[0144]

[0145] Table 9 Moisture retention rate of hydrogel wet chamber lenses for dry eye prepared in Examples 1-26 sealed in a body temperature environment (37°C)

[0146]

[0147] From the analysis of Tables 1 to 6 above, it can be seen that for different embodiments, when the hydrogel coating contains three components of polyvinyl alcohol, sodium polyacrylate and nanocellulose, the water loss rate of the hydrogel coating is significantly lower than the water loss rate when there are only two or one components. This is because the three components improve the water absorption and water retention properties in different ways. Both polyvinyl alcohol and nanocellulose contain a large number of hydroxyl (-OH) groups, which can be combined with water molecules through hydrogen bonds, and sodium polyacrylate is an ionic hydrogel that can absorb a large amount of water through ion exchange and osmotic pressure. Sodium polyacrylate and polyvinyl alcohol may undergo physical or chemical cross-linking during the composite process to form a synergistic effect and form a more complex and stable network structure. This network structure can not only accommodate more water, but also effectively prevent the loss of water, thereby improving water retention. Nanocellulose has an extremely high specific surface area and can provide more sites for adsorbing water, greatly increasing the water absorption capacity of the hydrogel coating. At the same time, the addition of nanocellulose can form more micropores and nanopores in the hydrogel coating, improving the porosity of the material. These pores can accommodate more water molecules and further improve the water absorption capacity. Therefore, when the ratio of the three components is 1:1:1, the water absorption and water retention properties of the hydrogel coating are optimal.

[0148] From the analysis of Tables 7 to 9 above, it can be seen that for different embodiments, different preparation processes have no significant effect on the long-term moisturizing effect of the hydrogel coating, and only affect the rate of increase of ambient humidity in a short period of time. This is because hydrogel is a polymer with a three-dimensional network structure with a high water content. Although there are certain differences in components and internal structures, they all have the performance characteristics of being able to spontaneously dissipate moisture to the surrounding environment.

[0149] In order to verify the relevant properties of the hydrogel wet chamber lens 1-26 for dry eye prepared in Examples 1-26, characterization tests were performed on the prepared hydrogel wet chamber lens 1-26 for dry eye. The test results are as follows: Figures 1 to 6 shown. Figure 1 This is a schematic diagram of the structure of the hydrogel wet room mirror prepared in Example 7. Figure 2 This is a photograph of the hydrogel prepared in Example 7 adhered to PMMA. Figure 3 This is a photograph of the polyvinyl alcohol hydrogel prepared in Example 20 adhered to ABS. Figure 4 This is the water loss rate of the hydrogel wet chamber lens for dry eye prepared in Example 7 in an open environment. Figure 5 This is the water loss rate of the hydrogel wet chamber lens for dry eye prepared in Example 7 in a closed environment. Figure 6 This is the moisture retention rate of the hydrogel wet chamber lens for dry eye prepared in Example 7 in a closed environment.

[0150] according to Figure 2 and Figure 3It can be seen that the frames modified by surface activation, whether PMMA or ABS, can be well grafted with hydrogel materials on the surface, making them adhere to the surface to provide a long-term moist environment.

[0151] according to Figure 4 and Figure 5 It can be seen that the hydrogel wet chamber lens used for dry eye quickly evaporates and loses water in an open environment, but can keep the water non-volatile for a long time in a closed environment.

[0152] according to Figure 6 It can be seen that the hydrogel wet chamber lens for dry eye can quickly increase the humidity of the environment and maintain it for a long time in a closed environment. This shows that the hydrogel wet chamber lens for dry eye prepared by the present invention can lock moisture for a long time, maintain high humidity in a closed environment, and thus effectively treat dry eye.

[0153] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a hydrogel wet chamber lens for dry eye, characterized in that: include: Dissolve polyvinyl alcohol in 95°C water to form solution A; dissolve sodium polyacrylate in water to form solution B; disperse nanocellulose in water to form suspension C; dissolve tris(hydroxymethyl)aminomethane in water and adjust the pH to form solution D; Dissolving dopamine in the solution D to obtain a solution E; Immersing the frame in the solution E, performing surface activation modification, washing, and drying, and collecting the modified frame; The modified frame is immersed in a mixed solution of the solution A, the solution B and the suspension C, and subjected to multiple freeze-thaw cycles, and the frame with the hydrogel moisturizing coating is collected to obtain a hydrogel wet chamber lens for dry eye.

2. The method for preparing the hydrogel wet chamber lens for dry eye according to claim 1, characterized in that: The content of polyvinyl alcohol in the solution A is 15wt%; And / or, the concentration of sodium polyacrylate in the solution B is 15wt%; and / or, the concentration of nanocellulose in the solution C is 15 wt %; And / or, the concentration of tris(hydroxymethyl)aminomethane in the solution D is 10 mmol / L; And / or, the concentration of dopamine in the solution E is 2 mg / mL.

3. The method for preparing the hydrogel wet chamber lens for dry eye according to claim 1, characterized in that: The pH value of the solution B is 7.5-8.

5.

4. The method for preparing the hydrogel wet chamber lens for dry eye according to claim 1, characterized in that: The thickness of the hydrogel moisturizing coating is 3 to 4 mm.

5. The method for preparing the hydrogel wet chamber lens for dry eye according to claim 1, characterized in that: The polyvinyl alcohol is 1797 type polyvinyl alcohol.

6. The method for preparing the hydrogel wet chamber lens for dry eye according to claim 1, characterized in that: When the polyvinyl alcohol is dissolved in 95°C water, the dissolution time is 2 hours; And / or, when the sodium polyacrylate is dissolved in water, the dissolution time is 2 hours; And / or, the nanocellulose is dispersed in water for 2 hours.

7. The method for preparing the hydrogel wet chamber lens for dry eye according to claim 1, characterized in that: When the modified base plate is immersed in the mixed solution of the solution A, the solution B and the suspension C, the immersion temperature is 27° C. and the immersion time is 24 hours.

8. The method for preparing the hydrogel wet chamber lens for dry eye according to claim 1, characterized in that: When the multiple freezing cycles are performed, the freezing time is 8 hours; And / or, when the hydrogel moisturizing coating is thawed, the thawing time is 4 hours.

9. A hydrogel wet chamber lens for dry eye prepared by the method according to any one of claims 1 to 8.

10. Use of a hydrogel wet chamber lens for dry eye prepared by the method of any one of claims 1 to 8 or a hydrogel wet chamber lens for dry eye according to claim 9 in the treatment of dry eye.