Super-wettability self-gelation styptic powder and preparation method thereof
By replacing sodium ions with calcium, strontium, copper, and cerium ions in the self-gelized hemostatic powder, improving its infiltration and water absorption ability, the problem of insufficient hemostatic effect of existing hemostatic powder under hypertension conditions is solved, and the problem of insufficient hemostatic effect of existing hemostatic powder under hypertension conditions is achieved. Efficient hemostasis and good biodegradability.
Patent Information
- Application Number
- CN202411130489.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
The existing self-gelized hemostatic powder is insufficiently wet, which makes it difficult to form a dense gel layer in the blood and cannot effectively block blood flow. Especially in the case of large blood pressure, the hemostatic effect is poor.
The sodium ions in sodium carboxymethylcellulose are replaced by high-valent metal ions such as calcium, strontium, copper, and cerium through ion exchange method, which increases its contact angle with water, makes it super-immersive, thereby enhancing water absorption and self-coagulation Geling ability and tissue adhesion form high density hydrogels to achieve sealing and hemostatic.
It significantly improves the infiltration and tissue adhesion of hemostatic powder, can effectively block blood flow under hypertension, promote coagulation, and completely degrade in the animal body without secondary removal, and has efficient hemostatic effect and good tissue Compatibility.
Smart Images

Figure CN119015478A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medical devices, in particular to a super-wetting self-gelling hemostatic powder and a preparation method thereof. Background Art
[0002] Hemostatic powder is a commonly used hemostatic material in clinical practice. It has the characteristics of high specific surface area, small volume, and good fluidity, making it particularly suitable for narrow, slightly deep, irregular, and unknown bleeding sites. Traditional hemostatic powders, such as zeolite Chitosan (Celox TM ),starch Etc., mainly accelerate hemostasis by absorbing water and promoting coagulation; its particles lack adhesion and are difficult to adhere to the tissue surface to form an effective physical barrier to block blood flow, especially when the blood pressure is high, they are easily washed away by the blood flow, which greatly limits its hemostatic effect.
[0003] In recent years, self-gelling hemostatic powder has attracted much attention due to its strong sealing and hemostatic ability. After contacting blood, it can quickly absorb water to form a hydrogel in situ, adhere to the tissue surface, form a physical barrier, and seal and stop bleeding. The wettability of self-gelling hemostatic powder is a key factor affecting its water absorption and gelation process. Powders with poor wettability tend to float on the liquid surface, have a low degree of self-gelation, and the gel layer formed is difficult to effectively adhere to the tissue surface and lacks density, so it is difficult to exert a sealing and hemostatic effect.
[0004] Common water-soluble polysaccharide powders, such as sodium alginate, sodium hyaluronate, quaternized chitosan, sodium carboxymethyl cellulose, etc., can form a hydrogel layer through physical cross-linking at the interface in contact with water, but due to insufficient wettability, the gel layer floats on the liquid surface, and the gel thickness, density, water absorption and water absorption efficiency are not ideal. Although there are literature reports on the use of ion exchange method to introduce calcium ions into sodium carboxymethyl cellulose sponge to increase its procoagulant effect, the calcium ion content is low and the wettability is still insufficient, resulting in limited final hemostatic effect. Summary of the invention
[0005] In order to solve the above-mentioned problems of the prior art, the present invention provides a method for preparing a super-wettable self-gelling hemostatic powder, in which the sodium ions in sodium carboxymethyl cellulose are partially replaced by high-valent metal ions with stronger hydration ability such as calcium, strontium, copper, cerium, etc. through ion exchange, so that the prepared hemostatic powder has super-wettability, that is, its contact angle is close to 0° when it comes into contact with water, thereby greatly improving the water absorption self-gelling ability and tissue adhesion of the hemostatic powder, so that it can form a dense hydrogel in situ, adhere to the surface of bleeding tissue, and act as a physical barrier to achieve sealed hemostasis.
[0006] The present invention realizes a method for preparing a super-wetting self-gelling hemostatic powder through the following technical scheme, comprising the following steps:
[0007] Mix sodium carboxymethyl cellulose and the exchange solution, stir in a water bath, and prepare a suspension;
[0008] The suspension is centrifuged, washed, and then dried;
[0009] Wherein, in the exchange solution, the solute is selected from one or more of chlorides and nitrates containing calcium, strontium, copper or cerium ions, and the solvent is a mixture of water and ethanol in a mass ratio of (20-50):(50-80).
[0010] In one embodiment, the solvent is a mixture of water and ethanol in a mass ratio of (40-48):(52-60).
[0011] In one embodiment, the solvent is a mixture of water and ethanol in a mass ratio of (44-46):(54-56).
[0012] In one embodiment, in the exchange solution, the mass volume ratio of the solute is 1 g / 100 mL to 50 g / 100 mL.
[0013] In one embodiment, the washing is performed using the first solvent and the second solvent in sequence; the second solvent is ethanol.
[0014] In one embodiment, the temperature of the water bath stirring is 10°C to 60°C.
[0015] In one embodiment, the stirring time in the water bath is 0.5 h to 8 h.
[0016] In one embodiment, the drying temperature is 30°C to 80°C.
[0017] In one embodiment, the drying time is 3 hours to 24 hours.
[0018] The present invention also provides a super-wetting self-gelling hemostatic powder prepared by the above-mentioned preparation method.
[0019] The beneficial effect of the present invention is that, by limiting the ratio of water to ethanol in the exchange solvent, the present invention solves the problem of insufficient ion exchange efficiency in the process of preparing ion exchange carboxymethyl cellulose by ion exchange method, thereby solving the problem of insufficient wettability of self-gelling hemostatic powder, and greatly improving the wettability of ion exchange carboxymethyl cellulose powder to reach a super wettability level. In addition, the present invention partially replaces the sodium ions in sodium carboxymethyl cellulose with strontium, copper, and cerium ions, and the strontium, copper, and cerium ion exchange carboxymethyl cellulose hemostatic powder formed achieves the same or better wettability as calcium ion exchange carboxymethyl cellulose. The hemostatic powder designed by the present invention solves the problems of self-gelling hemostatic powder being unable to completely absorb interfacial liquid to form a dense gel to block bleeding sites, forming a thin hydrogel layer immediately when in contact with liquid to hinder hydration, and the formed gel being unable to be completely degraded by improving the wettability of the powder.
[0020] Furthermore, the hemostatic powder prepared by the preparation method of the present invention is a self-gelling powder with high tissue adhesion, the ability to promote blood coagulation and high hemostatic efficiency. The gel generated in situ by the powder can be completely degraded without the need for secondary removal. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A schematic diagram of the preparation method of the ion exchange carboxymethyl cellulose hemostatic powder provided by the present invention and its in vitro self-gelation process;
[0022] Figure 2 The microscopic morphology SEM photos of the sodium carboxymethyl cellulose and calcium ion exchange type carboxymethyl cellulose hemostatic powder provided by the present invention and the morphology and SEM microscopic morphology of the hydrogel formed after water absorption;
[0023] Figure 3 A diagram showing the in vitro liquid absorption and self-gelation process of the sodium carboxymethyl cellulose and calcium ion exchange type carboxymethyl cellulose hemostatic powder provided by the present invention;
[0024] Figure 4 This is a diagram showing the adhesion of sodium carboxymethyl cellulose, calcium ion exchange carboxymethyl cellulose, and cerium ion exchange carboxymethyl cellulose provided by the present invention to the surface tissue of pig skin coated with rhodamine-stained PBS;
[0025] Figure 5 This is a diagram showing the hemostatic effect of sodium carboxymethyl cellulose and calcium ion exchange type carboxymethyl cellulose provided by the present invention in a rabbit liver bleeding model;
[0026] Figure 6 This is a diagram showing the hemostatic effect of sodium carboxymethyl cellulose and calcium ion exchange type carboxymethyl cellulose hemostatic powder provided by the present invention in a rabbit middle ear artery bleeding model;
[0027] Figure 7The invention discloses a self-gelling condition of the calcium ion exchange type carboxymethyl cellulose hemostatic powder, the cerium ion exchange type carboxymethyl cellulose hemostatic powder, the strontium ion exchange type carboxymethyl cellulose hemostatic powder and the copper ion exchange type carboxymethyl cellulose hemostatic powder provided by the present invention at a powder-liquid volume ratio of 1:5. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0029] like Figure 1 As shown, the present invention provides a method for preparing a super-wetting self-gelling hemostatic powder, comprising the following steps:
[0030] Mix sodium carboxymethyl cellulose and the exchange solution, stir in a water bath, and prepare a suspension;
[0031] The suspension was centrifuged, washed, and then dried;
[0032] Wherein, in the exchange solution, the solute is selected from one or more of chlorides and nitrates containing calcium, strontium, copper or cerium ions, and the solvent is a mixture of water and ethanol in a mass ratio of (20-50):(50-80).
[0033] The inventors have found that by limiting the ratio of water to ethanol in the exchange solvent, the content of calcium ions in the calcium ion exchange type carboxymethyl cellulose can be effectively regulated. When the mass ratio of water to ethanol in the solvent is (20-50): (50-80), the calcium content in the prepared calcium ion exchange type carboxymethyl cellulose exceeds 3wt%, so that the calcium ion exchange type carboxymethyl cellulose has super wettability and retains self-gelling ability.
[0034] The inventors have also found that by partially replacing the sodium ions in sodium carboxymethyl cellulose with strontium, copper, or cerium ions, the sodium carboxymethyl cellulose can have the same super wettability as calcium ion exchange type carboxymethyl cellulose with a high calcium content and retain the self-gelling ability.
[0035] The advantages brought by super wettability include: (1) enabling the material to quickly absorb blood between it and the tissue, greatly improving the adhesion between the material and the tissue, enhancing the ability to seal the wound, and improving the hemostatic effect; (2) allowing blood to continuously and rapidly enter the hemostatic powder, quickly aggregating blood cells and platelets to form blood clots to promote hemostasis; (3) expanding the water absorption range and having better water absorption and gelation properties; (4) the hydrogel formed by in situ gelation has higher strength and can withstand higher blood pressure, expanding the application range of hemostatic powder.
[0036] The invention solves the problem of insufficient ion exchange efficiency in the process of preparing ion exchange carboxymethyl cellulose by an ion exchange method, thereby solving the problem of insufficient wettability of self-gelling hemostatic powder, and greatly improves the wettability of ion exchange carboxymethyl cellulose powder to reach a super wettability level.
[0037] The present invention has found that strontium, copper and cerium ion-exchanged carboxymethyl cellulose also has a super wettability level.
[0038] The calcium ion exchange type carboxymethyl cellulose hemostatic powder prepared by the invention has good biodegradability and tissue compatibility. In an animal body, it can be completely degraded in 14 days. At the same time, the overall inflammatory response of the wound is low, and the granulation tissue layer generated is denser and thinner, showing good tissue compatibility.
[0039] In a more specific example, the solvent is a mixture of water and ethanol in a mass ratio of 35:65.
[0040] In a specific example, the solvent is a mixture of water and ethanol in a mass ratio of (40-48):(52-60).
[0041] In a specific example, the solvent is a mixture of water and ethanol in a mass ratio of (44-46):(54-56).
[0042] In a more specific example, the solvent is a mixture of water and ethanol in a mass ratio of 45:55.
[0043] In a specific example, in the exchange solution, the mass volume ratio of the solute is 1g / 100mL to 50g / 100mL. It can be understood that in the present invention, the mass volume ratio of the solute includes but is not limited to 1g / 100mL, 5g / 100mL, 10g / 100mL, 15g / 100mL, 20g / 100mL, 25g / 100mL, 30g / 100mL, 35g / 100mL, 40g / 100mL, 45g / 100mL, and 50g / 100mL.
[0044] In a specific example, the washing is performed using a first solvent and a second solvent in sequence; the second solvent is ethanol.
[0045] In a specific example, the number of washings is three times. More specifically, the washing is firstly performed twice with the first solvent and then once with ethanol.
[0046] In a specific example, the temperature of the water bath stirring is 10° C. to 60° C. It can be understood that in the present invention, the temperature of the water bath stirring includes but is not limited to 10° C., 15° C., 20° C., 25° C., 30° C., 33° C., 34° C., 35° C., 36° C., 37° C., 38° C., 39° C., 40° C., 45° C., 50° C., 55° C., and 60° C.
[0047] In a specific example, the duration of water bath stirring is 0.5h to 8h. It can be understood that in the present invention, the duration of water bath stirring includes but is not limited to 0.5h, 1h, 1.5h, 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h, 3.2h, 3.4h, 3.6h, 3.8h, 4h, 5h, 6h, 7h, and 8h.
[0048] In a specific example, the drying temperature is 30° C. to 80° C. It can be understood that in the present invention, the drying temperature includes but is not limited to 30° C., 35° C., 40° C., 45° C., 50° C., 55° C., 56° C., 57° C., 58° C., 59° C., 60° C., 61° C., 62° C., 63° C., 64° C., 65° C., 70° C., 75° C., and 80° C.
[0049] In a specific example, the drying time is 3 hours to 24 hours. It can be understood that in the present invention, the drying time includes but is not limited to 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours, and 24 hours.
[0050] The self-gelling absorbable hemostatic powder and its preparation method of the present invention are further described in detail below in conjunction with specific examples. The raw materials used in the following examples are all commercially available products unless otherwise specified.
[0051] Example 1
[0052] This embodiment provides a method for preparing a super-wetting self-gelling hemostatic powder, which is as follows:
[0053] Prepare an ethanol / water solution with a mass ratio of 55:45;
[0054] Sodium carboxymethylcellulose powder was suspended in an ethanol / water solution containing calcium chloride (15% w / v), and then stirred in a 37°C water bath for 3 hours. The resulting suspension was centrifuged, washed twice with an ethanol / water solvent, and once with ethanol. Finally, after drying at 60°C overnight, the target hemostatic powder was obtained.
[0055] Example 2
[0056] This embodiment provides a method for preparing a super-wetting self-gelling hemostatic powder, which is as follows:
[0057] Prepare an ethanol / water solution with a mass ratio of 65:35;
[0058] Sodium carboxymethylcellulose powder was suspended in an ethanol / water solution containing calcium chloride (15% w / v), and then stirred in a 37°C water bath for 3 hours. The resulting suspension was centrifuged, washed twice with an ethanol / water solvent, and once with ethanol. Finally, after drying at 60°C overnight, the target hemostatic powder was obtained.
[0059] Example 3
[0060] This embodiment provides a method for preparing a super-wetting self-gelling hemostatic powder, which is as follows:
[0061] Prepare an ethanol / water solution with a mass ratio of 45:55;
[0062] Sodium carboxymethylcellulose powder was suspended in an ethanol / water solution containing cerium chloride (15 wt%) and then stirred in a 37°C water bath for 2 hours. The resulting suspension was centrifuged, washed twice with an ethanol / water solvent and once with ethanol. Finally, after drying at 70°C overnight, the target hemostatic powder was obtained.
[0063] Example 4
[0064] This embodiment provides a method for preparing a super-wetting self-gelling hemostatic powder, which is as follows:
[0065] Prepare an ethanol / water solution with a mass ratio of 45:55;
[0066] Sodium carboxymethylcellulose powder was suspended in an ethanol / water solution containing strontium nitrate (15 wt%) and then stirred in a 37°C water bath for 4 hours. The resulting suspension was centrifuged, washed twice with an ethanol / water solvent and once with ethanol. Finally, after drying at 60°C overnight, the target hemostatic powder was obtained.
[0067] Example 5
[0068] This embodiment provides a method for preparing a super-wetting self-gelling hemostatic powder, which is as follows:
[0069] Prepare an ethanol / water solution with a mass ratio of 55:45;
[0070] Sodium carboxymethylcellulose powder was suspended in an ethanol / water solution containing copper chloride (5 wt%) and then stirred in a 37°C water bath for 2 hours. The resulting suspension was centrifuged, washed twice with an ethanol / water solvent and once with ethanol. Finally, after drying at 70°C overnight, the target hemostatic powder was obtained.
[0071] Comparative Example 1
[0072] This comparative example provides a method for preparing a super-wetting self-gelling hemostatic powder, which is as follows:
[0073] Prepare an ethanol / water solution with a mass ratio of 20:80;
[0074] Sodium carboxymethylcellulose powder was suspended in an ethanol / water solution containing calcium chloride (15 w / v), and then stirred in a 37°C water bath for 3 hours. The resulting suspension was centrifuged, washed twice with an ethanol / water solvent, and once with ethanol. Finally, after drying at 60°C overnight, the target hemostatic powder was obtained.
[0075] Effect verification test
[0076] The hemostatic powders prepared in the above-mentioned Example 1, Example 2, Example 3 and Comparative Example 1 were subjected to effect verification experiments.
[0077] The calcium content of the calcium ion exchange carboxymethyl cellulose prepared in Example 1 was 5.59% as determined by ICP and EDS, the calcium content of the calcium ion exchange carboxymethyl cellulose prepared in Example 2 was 3.15%, and the calcium content of the calcium ion exchange carboxymethyl cellulose prepared in Comparative Example 1 was 1.78%. When the calcium content exceeds 3wt%, the calcium ion exchange carboxymethyl cellulose can have super wettability. The cerium content of the cerium ion exchange carboxymethyl cellulose prepared in Example 3 was 4% as determined by ICP and EDS.
[0078] like Figure 2 As shown, the calcium ion exchange type carboxymethyl cellulose of the present invention is in the form of relatively short fibers under microscopic conditions, the fiber surface is relatively rough, and calcium is mostly distributed on the fiber surface, showing the characteristics of being dense near the surface and sparse near the core, while the distribution of sodium is just the opposite. At the same time, the ion exchange method does not affect the polymer chain structure of carboxymethyl cellulose and has little effect on its electronegativity (the Zeta potential of sodium carboxymethyl cellulose is -29.5mV, and the Zeta potential of calcium ion exchange type carboxymethyl cellulose with a calcium content of 5.59% is -25.0mV).
[0079] The calcium ion exchange type carboxymethyl cellulose powder and the cerium ion exchange type carboxymethyl cellulose powder prepared by sodium carboxymethyl cellulose powder, Example 1, Example 2, Example 3 and Comparative Example 1 were compressed into sheets under a pressure of 2.5 MPa and their wettability was measured by water contact angle. The water contact angles of sodium carboxymethyl cellulose were 45.2°, respectively, and the water contact angles of Examples 1, 2 and 3 were close to 0°, showing super wettability, and the water contact angles of Comparative Example 1 were 33.2°. In addition, its wettability increased with the increase of calcium content.
[0080] like Figure 3 As shown, sodium carboxymethylcellulose powder and the hemostatic powder prepared in Example 1 and Example 2 are sprinkled on the surface of liquid (the water excess is 1 / 10 powder-liquid ratio, w / v; the powder excess is 1 / 1 powder-liquid ratio, w / v). The calcium ion exchange type carboxymethylcellulose powder can quickly and completely absorb the liquid to form a gel, but sodium carboxymethylcellulose only forms a thin layer of gel at the interface where the liquid and powder contact. This thin layer of gel hinders further hydration of the powder. Further increasing the powder-to-liquid ratio, sodium carboxymethylcellulose powder still forms a similar thin gel layer, which shows that the degree of in-situ gelation of sodium carboxymethylcellulose has nothing to do with its usage. Figure 7 Shown are the self-gelation conditions of the calcium ion exchange carboxymethyl cellulose hemostatic powder provided in Example 2 of the present invention and the cerium ion exchange carboxymethyl cellulose hemostatic powder provided in Example 3 at a powder-to-liquid volume ratio of 1:5, as well as the gel morphology after the gel is sprinkled in excess water to form a bottom, adhere to the beaker wall and peel off.
[0081] The water absorption rate of the calcium ion exchange carboxymethyl cellulose prepared in Example 1 of the present invention is in the range of 184-2010%, the water absorption rate of the calcium ion exchange carboxymethyl cellulose prepared in Example 2 is in the range of 211-1543%, and the water absorption rate of the cerium ion exchange carboxymethyl cellulose prepared in Example 3 is in the range of 147-2345%, which is significantly larger than the 929-1013% of sodium carboxymethyl cellulose and has a better water absorption effect.
[0082] The calcium ion exchange carboxymethyl cellulose prepared in Example 1 and Example 2 has a fast swelling rate and can be completely dissolved after being soaked in water for 8 hours.
[0083] like Figure 4As shown, when sodium carboxymethylcellulose, blood powder obtained in Example 1, Example 2 and Example 3 are sprinkled on pigskin coated with PBS, the hydrogel formed in situ adheres tightly to the pigskin and can withstand bending, twisting, washing and other operations without falling off, and its adhesion stress can reach up to 10.9 kPa (calcium ion exchange type carboxymethylcellulose) and 17.6 kPa (cerium ion exchange type carboxymethylcellulose). However, sodium carboxymethylcellulose has insufficient wettability, a large amount of powder floats, and the material falls off after rotating the pigskin, and the tissue adhesion is insufficient, and its adhesion stress is only 2.5 kPa.
[0084] The procoagulant activity of calcium ion exchange carboxymethyl cellulose increases with the increase of its calcium content. It can completely form a stable blood clot after mixing with blood in vitro for 4 minutes. The procoagulant activity of cerium ion exchange carboxymethyl cellulose is slightly worse than that of calcium ion exchange carboxymethyl cellulose, and it can completely form a stable blood clot in about 6 minutes.
[0085] In an animal model of liver bleeding with relatively low blood pressure, calcium ion exchange carboxymethyl cellulose hemostatic powder and cerium ion exchange carboxymethyl cellulose hemostatic powder with super wettability can quickly and completely absorb the blood lost from the wound to form a hydrogel barrier with super high tissue adhesion, which physically blocks the wound site to achieve a hemostatic effect. The hemostatic effect can be seen immediately when calcium ion exchange carboxymethyl cellulose hemostatic powder is sprinkled on the wound surface, and it can completely stop bleeding within 5 minutes without pressure. The hydrogel barrier formed has a good wound sealing effect. Figure 5 As shown, when the calcium content of the hemostatic powder prepared in Example 1 reaches 5.59%, the gel formed can be completely peeled off from the wound without causing secondary bleeding, while when the calcium content of the hemostatic powder prepared in Example 2 is reduced relative to that of Example 1, only part of the gel can be peeled off. The hemostatic effect of sodium carboxymethyl cellulose powder is poor, and there is no obvious blood loss in the first 1 minute after contacting the wound, but blood gushes out of the powder afterwards.
[0086] like Figure 6 As shown, in the rabbit middle auricular artery injury animal model with high blood pressure and large bleeding volume, the calcium ion exchange type carboxymethyl cellulose prepared in Example 1 can stop bleeding within 5 minutes without applying additional pressure, and there is no secondary bleeding after the gel is removed; the calcium ion exchange type carboxymethyl cellulose prepared in Example 2 can stop bleeding but secondary bleeding occurs after the gel is removed; while sodium carboxymethyl cellulose fails to block, and blood breaks through the barrier.
[0087] In the animal body, the hemostatic powder prepared in Example 1 and Example 2 can be completely degraded in 14 days. At the same time, the overall inflammatory response of the wound is low, and the granulation tissue layer generated is denser and thinner, showing better tissue compatibility.
[0088] like Figure 7As shown, the calcium ion exchange carboxymethyl cellulose prepared in Example 2, the cerium ion exchange carboxymethyl cellulose prepared in Example 3, the strontium ion exchange carboxymethyl cellulose prepared in Example 4, and the copper ion exchange carboxymethyl cellulose prepared in Example 5 can all quickly absorb liquid at a powder-liquid volume ratio of 1:5 to form a uniform, complete hydrogel with a certain strength. Among them, the water absorption rate of Example 5 is slightly lower, and residual unabsorbed liquid can be seen, while the other examples all completely absorb the liquid.
[0089] In the description of the embodiments of the present invention, the terms "first", "second", "third", and "fourth" are used for descriptive purposes only and are not to be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", "third", and "fourth" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0090] In the description of the embodiments of the present invention, it is to be understood that "-" and "~" represent the range between two values, and the range includes the endpoints. For example: "AB" represents a range greater than or equal to A and less than or equal to B. "A~B" represents a range greater than or equal to A and less than or equal to B.
[0091] In the description of the embodiments of the present invention, the term "and / or" herein is merely a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " herein generally indicates that the associated objects before and after are in an "or" relationship.
[0092] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a super-wetting self-gelling hemostatic powder, characterized in that: The steps include: Mix sodium carboxymethyl cellulose and the exchange solution, stir in a water bath, and prepare a suspension; The suspension is centrifuged, washed, and then dried; Wherein, in the exchange solution, the solute is selected from one or more of chlorides and nitrates containing calcium, strontium, copper or cerium ions, and the solvent is a mixture of water and ethanol in a mass ratio of (20-50):(50-80).
2. The method for preparing the super-wetting self-gelling hemostatic powder according to claim 1, characterized in that: The solvent is a mixture of water and ethanol in a mass ratio of (40-48):(52-60).
3. The method for preparing the super-wetting self-gelling hemostatic powder according to claim 2, characterized in that: The solvent is a mixture of water and ethanol in a mass ratio of (44-46):(54-56).
4. The method for preparing the super-wetting self-gelling hemostatic powder according to claim 1, characterized in that: In the exchange solution, the mass volume ratio of the solute is 1 g / 100 mL to 50 g / 100 mL.
5. The method for preparing the super-wetting self-gelling hemostatic powder according to claim 1, characterized in that: The first solvent and the second solvent are used successively for washing; the second solvent is ethanol.
6. The method for preparing the super-wetting self-gelling hemostatic powder according to claim 1, characterized in that: The temperature of the water bath stirring is 10°C to 60°C.
7. The method for preparing the super-wetting self-gelling hemostatic powder according to claim 1, characterized in that: The stirring time in the water bath is 0.5h to 8h.
8. The method for preparing the super-wetting self-gelling hemostatic powder according to any one of claims 1 to 7, characterized in that: The drying temperature is 30°C to 80°C.
9. The method for preparing the super-wetting self-gelling hemostatic powder according to any one of claims 1 to 7, characterized in that: The drying time is 3h to 24h.
10. Super wettability self-gelling hemostatic powder prepared by the preparation method according to any one of claims 1 to 9.