Vacuum heat insulation polyether-ether-ketone composite conduit and preparation method thereof

By using a three-layer polyether ether ketone material, the heat resistance and heat insulation of the composite catheter in high temperature environments is solved, achieving a longer service life and higher therapeutic efficiency.

CN119015572AInactive Publication Date: 2024-11-26NINGBO LINSTANT POLYMER MATERIALS CO LTD

Patent Information

Application Number
CN202411501977.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing composite catheters have poor heat resistance and heat insulation when used in high temperature environments, which can easily lead to scalding of the catheter itself and contact with external tissues, and have a short service life.

Method used

The vacuum insulation composite conduit design using three-layer polyether ether ketone material includes inner tube, intermediate braided tube and outer tube. The intermediate braided tube is formed by three-dimensional braided and heat-shrinked covering the outer tube on its outside to form a vacuum Insulating chambers to improve high temperature resistance and thermal insulation performance.

Benefits of technology

It significantly improves the high temperature and drug resistance of the composite catheter, extends its service life, ensures that high temperature treatment is only concentrated in the treatment area, reduces damage to healthy tissues, and improves the flexibility and deformation resistance of the catheter.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119015572A_ABST
    Figure CN119015572A_ABST
Patent Text Reader

Abstract

The invention discloses a vacuum heat-insulation polyether-ether-ketone composite conduit and a preparation method thereof.The vacuum heat-insulation polyether-ether-ketone composite conduit comprises an inner-layer pipe, an outer-layer pipe and a middle braided pipe arranged between the inner-layer pipe and the outer-layer pipe, the inner-layer pipe, the middle braided pipe and the outer-layer pipe are all made of polyether-ether-ketone, the middle braided pipe is tightly wrapped with the outer-layer pipe, and the outer-layer pipe is tightly wrapped with the middle braided pipe. The two ends of the outer-layer pipe and the two ends of the inner-layer pipe are connected in a sealed mode, and a vacuum heat insulation cavity is formed between the outer-layer pipe and the inner-layer pipe. The composite catheter has the advantages of being good in high-temperature resistance and drug resistance, improving the heat preservation effect in the composite catheter, effectively insulating heat between the interior of the composite catheter and the external environment and prolonging the service life of the composite catheter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical devices, and in particular to a vacuum-insulated polyetheretherketone composite catheter and a preparation method thereof. Background Art

[0002] Some treatment techniques need to be performed in a high-temperature environment. These techniques are usually called hyperthermia. Common application scenarios of hyperthermia include cancer treatment, cardiovascular disease treatment, and other treatment scenarios that require local heating, such as cardiac ablation. Cardiac ablation is used to treat arrhythmias and destroy abnormal cardiac tissue through local heating. In summary, hyperthermia can kill cancer cells by heating the temperature of local tissue to achieve a therapeutic effect. Thermal chemotherapy is the combination of chemotherapy drugs and hyperthermia. Its principle is to use physical energy to heat chemotherapy drugs with good thermal effects, thereby raising the temperature of tumor tissue to an effective treatment temperature and maintaining it for a certain period of time. The difference in temperature tolerance between normal tissues and tumor cells is used to achieve the therapeutic purpose of causing tumor cell apoptosis. However, in the above-mentioned treatments involving heat therapy or thermochemotherapy, it is usually necessary to first implant a composite catheter into the body and directly reach the lesion site, and then introduce the interventional medical device or high-temperature fluid from the lumen of the composite catheter into the lesion site for treatment. During the high-temperature treatment, it is necessary to ensure that the high temperature is only concentrated in the treatment area and does not spread to other healthy tissues. However, the heat resistance and heat insulation effects of the composite catheters on the market are not ideal, and the composite catheters themselves and human tissues that contact the outer wall of the composite catheters are prone to burns, which urgently needs to be improved. Summary of the invention

[0003] The purpose of the present invention is to provide a vacuum insulated polyetheretherketone composite conduit and a preparation method thereof, which has the effects of good high temperature resistance and drug resistance of the composite conduit, improving the thermal insulation effect inside the composite conduit, being able to effectively insulate the inside of the composite conduit from the external environment, and extending the service life of the composite conduit.

[0004] The above technical purpose of the present invention is achieved through the following technical scheme: a vacuum insulated polyetheretherketone composite conduit, comprising an inner tube, an outer tube and an intermediate braided tube arranged between the inner tube and the outer tube, the materials of the inner tube, the intermediate braided tube and the outer tube are all set to polyetheretherketone, the outer tube is tightly wrapped around the outside of the intermediate braided tube, and the outer tube is sealed and connected to both ends of the inner tube, and a vacuum insulation cavity is formed between the outer tube and the inner tube.

[0005] By adopting the above technical scheme, the polyetheretherketone material itself has high heat resistance, wear resistance and drug resistance, and the polyetheretherketone material also has good biocompatibility, and can be used as a long-term implant in the human body, thereby reducing tissue reaction and rejection, and is widely used in medical fields such as minimally invasive surgery, imaging catheters and long-term indwelling catheters. However, there is currently no composite catheter on the market in which the inner tube, the middle braided tube and the outer tube are simultaneously set to polyetheretherketone material. The present invention is beneficial to improving the overall high temperature resistance and drug resistance of the composite catheter by setting the inner tube, the middle braided tube and the outer tube to polyetheretherketone material at the same time. The composite catheter can withstand high temperature disinfection without decomposition, and can be suitable for the application of medical devices that need to be repeatedly disinfected by high temperature or drugs, thereby extending the service life of the composite catheter of the present invention; in addition, the composite catheter of the present invention is made of three layers of polyetheretherketone material, which can effectively increase the overall flexibility and deformation resistance of the composite catheter; at the same time, the composite catheter of the present invention forms a vacuum insulation cavity between the inner tube and the outer tube, and through the middle braided tube, a vacuum insulation cavity is formed between the inner tube and the outer tube. The woven tube supports the gap between the inner tube and the outer tube to prevent the outer tube from sticking to the surface of the inner tube. The vacuum insulation cavity formed between the inner tube and the outer tube can effectively isolate the heat transfer between the inner cavity of the inner tube and the external environment of the outer tube. For example, when high-temperature liquid or gas needs to be transmitted in the inner tube, the vacuum insulation cavity can ensure that the high temperature is only concentrated in the treatment area, and the heat will not be transferred to the outside of the composite catheter to damage other healthy tissues during the transmission process. At the same time, it can also improve the thermal insulation capacity of the inner tube, reduce the energy loss of the composite catheter when transferring heat, and ensure that the temperature required for treatment is maintained. In addition, the polyetheretherketone material also has high self-lubricity, which can reduce the friction between the composite catheter and the interventional medical device in the inner cavity, thereby improving the smoothness of the outer wall of the composite catheter when inserted into the human tissue, and the composite catheter has good high temperature resistance and drug resistance. It can not only improve the thermal insulation effect inside the composite catheter, but also effectively insulate the inside of the composite catheter from the external environment, and has the effect of extending the service life of the composite catheter.

[0006] The present invention is further configured as follows: the outer tube is configured as a polyetheretherketone heat shrink tube, and the outer tube is tightly coated on the outer wall of the middle braided tube through a heat shrink process.

[0007] By adopting the above technical solution, the outer tube can be shrunk by heating and tightly wrapped around the outside of the middle braided tube, thereby improving the convenience of installation of the outer tube.

[0008] The present invention is further configured as follows: the intermediate braided tube is formed by three-dimensionally braiding a plurality of polyetheretherketone fiber filaments outside the inner tube, and hollow mesh holes for air flow are formed between adjacent polyetheretherketone fiber filaments.

[0009] By adopting the above technical solution, the middle braided tube is formed by three-dimensional weaving, so that there are nodes that are folded and crossed up and down between adjacent polyetheretherketone fiber filaments, and the height of the nodes is higher than the height of a single polyetheretherketone fiber filament nearby, thereby forming a supporting space, so that when the outer tube is wrapped around the outside of the middle braided tube, airway gaps are formed between adjacent cross nodes, and multiple airway gaps are interconnected. After the air is extracted, a vacuum insulation cavity is formed between the outer tube and the inner tube.

[0010] The present invention is further configured as follows: the number of coaxial braiding layers of the intermediate braided tube is set to at least one layer.

[0011] By adopting the above technical solution, a larger number of braided layers can increase the thickness of the middle braided tube, thereby improving the pressure resistance; a smaller number of braided layers can enable the composite catheter to maintain better flexibility.

[0012] Another technical object of the present invention is to provide a method for preparing a vacuum insulated polyetheretherketone composite conduit, comprising the following steps: S1: Inner tube preparation, including the following steps: S101: Raw material preparation: Polyetheretherketone granules are selected as raw materials; S102: extrusion molding: heating the polyetheretherketone pellets to a melting point above 334°C, and extruding through an extruder to form a hollow inner tube; S103: Cooling and shaping: cooling and shaping the inner tube after extrusion in a cooling water tank; S104: Surface treatment: The outer wall of the inner tube is mechanically polished or the outer surface is treated with chemical reagents to enhance the bonding force between the outer surface of the inner tube and the middle braided tube; S2: Preparation of intermediate braided tube, including the following steps: S201: Raw material preparation: Polyetheretherketone fiber yarn is selected as the weaving material; S202: Weaving and forming: positioning the inner tube prepared in S1 on a three-dimensional weaving machine, weaving the polyetheretherketone fiber filaments on the outer wall of the inner tube by the three-dimensional weaving machine to form an intermediate braided tube; S3: outer tube preparation, including the following steps: S301: Raw material preparation: Polyetheretherketone heat shrink tubing is used as the material of the outer tube; S302: Sleeve connection: coaxially sleeve the polyetheretherketone heat shrink tube outside the middle braided tube; S303: heat shrinkage treatment: external heating is used to shrink the polyetheretherketone heat shrinkable tube inward to form an outer tube that fits closely with the outer surface of the middle braided tube; S304: Cooling and shaping: ensuring that the outer tube after heat shrinkage is completely cooled and shaped; S4: Formation of a vacuum insulation cavity, comprising the following steps: S401: vacuum preparation: blocking both ends of the composite conduit, and opening at least one vacuum hole for vacuuming on the blocked composite conduit; S402: Vacuuming treatment: using a vacuuming device to extract the air between the inner tube and the outer tube through the reserved air extraction holes, and supporting the gap between the inner tube and the outer tube through the middle braided tube, so that a vacuum heat insulation cavity is formed between the inner tube and the outer tube; S403: Sealing process: After the vacuuming is completed, the vacuum holes on the composite conduit are sealed to ensure that the composite conduit remains in a vacuum state; S404: Vacuum test: Perform vacuum pressure test on the vacuum insulation cavity of the composite conduit through pressure testing equipment to ensure that the vacuum insulation cavity of the composite conduit can maintain a vacuum state within a predetermined time to ensure that there is no leakage in the vacuum insulation cavity; S5: Post-processing: grinding and coating the outer surface of the composite catheter.

[0013] The present invention is further configured as follows: the diameter of the polyetheretherketone fiber filament in step S201 is set between 50-200 microns.

[0014] By adopting the above technical scheme, a smaller diameter of the polyetheretherketone fiber filament can improve the flexibility of the intermediate braided tube, and a larger diameter of the polyetheretherketone fiber filament can increase the structural strength of the intermediate braided tube. Therefore, setting the diameter of the polyetheretherketone fiber filament between 50-200 microns can ensure that the intermediate braided tube has good flexibility and a certain structural strength.

[0015] The present invention is further configured as follows: the braiding density of the polyetheretherketone fiber filaments of the intermediate braided tube in step S202 is set between 5 and 20 strands / cm.

[0016] By adopting the above technical solution, the middle braided tube has both high compressive resistance and structural strength and a certain degree of flexibility.

[0017] The present invention is further configured as follows: the three-dimensional braiding machine of the intermediate braided tube in step S202 is braided in one of plain weave, twill weave or satin weave.

[0018] By adopting the above technical scheme, different weaving patterns will affect the flexibility and compression resistance of the braided layer. Among them, the intermediate braided tube formed by plain weaving has better flexibility, while the intermediate braided tube formed by twill weaving and satin weaving has higher strength and compression resistance. Medical personnel can choose the composite catheter prepared by the corresponding weaving method according to the actual scene needs.

[0019] The present invention is further configured as follows: the plugging process in step S401 and the sealing process in step S403 are both performed by heat-melting or gluing at both ends of the inner tube and the outer tube, and the air extraction holes are opened on the corresponding heat-melting surfaces or glue bonding surfaces.

[0020] By adopting the above technical scheme, when the composite conduit is vacuum treated, the ends of the inner tube and the outer tube are first sealed by heat melting or glue bonding, and then an exhaust hole is opened on the heat melting surface or the glue bonding surface, and then a vacuum is drawn by a vacuum pumping device to form a vacuum insulation cavity. After the vacuuming is completed, the exhaust hole is sealed again by heat melting or glue bonding to achieve vacuum sealing of the vacuum insulation cavity.

[0021] The present invention is further configured as follows: the sealing treatment in step S401 is performed by heat melting or glue bonding at both ends of the inner tube and the outer tube, and the exhaust hole is opened on the outer wall of the outer tube; the sealing treatment in step S403 is performed by sleeved a layer of polyetheretherketone heat shrinkable tube on the outside of the outer tube in alignment with the exhaust hole, and the polyetheretherketone heat shrinkable tube is heated to shrink and wrap around the outside of the outer tube, and the exhaust hole is sealed.

[0022] By adopting the above technical scheme, when the composite conduit is vacuum treated, the ends of the inner tube and the outer tube are first sealed by heat melting or glue bonding, and then an exhaust hole is opened on the outer wall of the outer tube. After that, a vacuum is drawn using a vacuum pumping device to form a vacuum insulation cavity. After the vacuum is completed, a layer of polyetheretherketone heat shrinkable tube is sheathed on the outside of the outer tube, and the outermost layer of polyetheretherketone heat shrinkable tube is heat-shrunk and wrapped around the outer tube by heating, thereby achieving vacuum sealing of the vacuum insulation cavity.

[0023] In summary, the present invention has the following beneficial effects: The intermediate braided tube is formed by three-dimensional weaving outside the inner tube, and then the outer tube is heat-shrinkably coated outside the intermediate braided tube, wherein the materials of the inner tube, the intermediate braided tube and the outer tube are all set to polyetheretherketone, the two ends of the inner tube and the outer tube are sealed, and the space between the inner tube and the outer tube is evacuated to form a vacuum insulation cavity. The polyetheretherketone material itself has high heat resistance, wear resistance, drug resistance and biocompatibility, which can effectively increase the overall flexibility, deformation resistance, high temperature resistance and drug resistance of the composite catheter. In addition, the composite catheter of the present invention forms a vacuum insulation cavity between the inner tube and the outer tube, and supports the gap between the inner tube and the outer tube through the intermediate braided tube to prevent the outer tube from sticking to the surface of the inner tube; the vacuum insulation cavity formed between the inner tube and the outer tube can effectively isolate the inner cavity of the inner tube from the outer surface of the outer tube Heat transfer between the internal environment, for example, when high-temperature liquid or gas needs to be transmitted in the inner tube, the vacuum insulation cavity can ensure that the high temperature is only concentrated in the treatment area, and the heat will not be transferred to the outside of the composite catheter to damage other healthy tissues during the transmission process. At the same time, it can also improve the thermal insulation capacity of the inner tube, reduce the energy loss when the composite catheter transfers heat, and ensure that the temperature required for treatment is maintained; in addition, the polyetheretherketone material also has high self-lubricity, which can reduce the friction between the composite catheter and the interventional medical device in the inner cavity, thereby improving the smoothness of the outer wall of the composite catheter when inserted into the human tissue, and the composite catheter has good high temperature resistance and drug resistance. It can not only improve the thermal insulation effect inside the composite catheter, but also effectively insulate the inside of the composite catheter from the external environment, and has the effect of extending the service life of the composite catheter. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a diagram of the internal structure of the composite catheter of the present invention.

[0025] Figure 2 This is a view of a first specific embodiment of the present invention in which the air extraction holes are opened on the heat-melting surface or the glue bonding surface.

[0026] Figure 3 This is a view of a second specific embodiment of the present invention in which the exhaust holes are opened on the side wall of the outer tube, wherein the sealing tube has been wrapped and sealed on the corresponding exhaust holes after heat shrinkage.

[0027] In the figure: 1. Inner tube; 2. Middle braided tube; 2a. Hollow mesh; 21. Polyetheretherketone fiber; 3. Outer tube; a. Vacuum insulation cavity; b. Air extraction hole; 4. Sealing tube; 5. Hot-melt surface or glue bonding surface. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with the accompanying drawings. Specific embodiment 1 A vacuum insulated polyetheretherketone composite conduit, such as Figure 1-Figure 2As shown, it includes an inner tube 1, an outer tube 3 and an intermediate braided tube 2 arranged between the inner tube 1 and the outer tube 3. The materials of the inner tube 1, the intermediate braided tube 2 and the outer tube 3 are all set to polyetheretherketone. The outer tube 3 is tightly wrapped around the outside of the intermediate braided tube 2, and the outer tube 3 is sealed and connected to the inner tube 1 at both ends, and a vacuum insulation cavity a is formed between the outer tube 3 and the inner tube 1; the outer tube 3 is set to a polyetheretherketone heat shrinkable tube, and the outer tube 3 is tightly wrapped around the outer wall of the intermediate braided tube 2 through a heat shrinkage process, so that the outer tube 3 can shrink by heating and tightly wrap around the outside of the intermediate braided tube 2, thereby improving the installation convenience of the outer tube 3; the intermediate braided tube 2 is formed by three-dimensional weaving of a plurality of polyetheretherketone fiber filaments 21 outside the inner tube 1, and hollow mesh holes 2a for airflow are formed between adjacent polyetheretherketone fiber filaments 21. The intermediate braided tube 2 is formed by three-dimensional weaving, so that adjacent There are nodes between the polyetheretherketone fiber filaments 21 that are folded and crossed up and down, and the height of the nodes is higher than the height of the nearby single polyetheretherketone fiber filaments 21, thereby forming a supporting space, so that when the outer tube 3 is wrapped around the outside of the middle braided tube 2, airway gaps are formed between adjacent cross nodes, and multiple airway gaps are interconnected. After the air is extracted, a vacuum insulation cavity a is formed between the outer tube 3 and the inner tube 1; in this embodiment, the number of coaxial braiding layers of the middle braided tube 2 is set to one layer, so that the composite conduit of this embodiment has both flexibility and pressure resistance. In other embodiments, the number of braiding layers can be set to at least two layers. The number of braiding layers of the middle braided tube 2 is set to multiple layers, so that the hollow mesh holes 2a between adjacent braided layers can be interconnected, thereby improving the vacuum efficiency during vacuuming, improving the vacuuming effect, and being able to improve the overall flexibility and deformation resistance of the composite conduit.

[0030] The basic working principle of the present invention is: three-dimensionally weave the inner tube 1 to form an intermediate braided tube 2, and then heat shrink the outer tube 3 on the outer side of the intermediate braided tube 2, wherein the materials of the inner tube 1, the intermediate braided tube 2 and the outer tube 3 are all set to polyetheretherketone, the two ends of the inner tube 1 and the outer tube 3 are sealed, and the space between the inner tube 1 and the outer tube 3 is evacuated to form a vacuum insulation cavity a, and the polyetheretherketone material itself has high heat resistance, wear resistance and drug resistance, and the polyetheretherketone material also has good biocompatibility, and can be used as a long-term implant in the human body, thereby reducing tissue reaction and rejection, and is widely used in minimally invasive surgery. , imaging catheters and long-term indwelling catheters, etc. However, there is no composite catheter in the market that has the inner tube 1, the middle braided tube 2 and the outer tube 3 all made of polyetheretherketone. The present invention has the inner tube 1, the middle braided tube 2 and the outer tube 3 all made of polyetheretherketone, which is beneficial to improving the overall high temperature resistance and drug resistance of the composite catheter. It can withstand high temperature disinfection without decomposition, and can be suitable for the application of medical devices that need to be repeatedly disinfected by high temperature or drugs, thereby extending the service life of the composite catheter of the present invention. In addition, the composite catheter of the present invention is made of three-layer polyetheretherketone material, which can effectively increase The composite catheter has overall flexibility and deformation resistance; at the same time, the composite catheter of the present invention forms a vacuum insulation cavity a between the inner tube 1 and the outer tube 3, and supports the gap between the inner tube 1 and the outer tube 3 through the intermediate braided tube 2 to prevent the outer tube 3 from sticking to the surface of the inner tube 1. The vacuum insulation cavity a formed between the inner tube 1 and the outer tube 3 can effectively isolate the heat transfer between the inner cavity of the inner tube 1 and the external environment of the outer tube 3. For example, when high-temperature liquid or gas needs to be transmitted in the inner tube 1, the vacuum insulation cavity a can ensure that the high temperature is only concentrated in the treatment area, and the heat will not be transferred to the composite catheter during the transmission process. The composite catheter can not only prevent other healthy tissues from being damaged by the outside, but also improve the thermal insulation capacity of the inner layer tube 1, reduce the energy loss when the composite catheter transfers heat, and ensure that the temperature required for treatment is maintained; in addition, the polyetheretherketone material also has high self-lubricity, which can reduce the friction between the composite catheter and the interventional medical device in the inner cavity, thereby improving the smoothness of the outer wall of the composite catheter when inserted into human tissue, and has the effect of good high temperature resistance and drug resistance of the composite catheter, which can not only improve the thermal insulation effect inside the composite catheter, but also effectively insulate the inside of the composite catheter from the external environment, and has the effect of extending the service life of the composite catheter.

[0031] This embodiment provides a method for preparing a vacuum insulated polyetheretherketone composite conduit, comprising the following steps: S1: Preparation of inner layer tube 1, including the following steps: S101: Raw material preparation: Polyetheretherketone granules are selected as raw materials; S102: extrusion molding: heating the polyetheretherketone pellets to a melting point of 334° C. or higher, and extruding through an extruder to form a hollow inner tube 1; S103: Cooling and shaping: cooling and shaping the inner tube 1 after extrusion in a cooling water tank; S104: Surface treatment: mechanically grinding or treating the outer surface of the inner tube 1 with chemical reagents to enhance the bonding force between the outer surface of the inner tube 1 and the middle braided tube 2; S2: Preparation of the intermediate braided tube 2, including the following steps: S201: Raw material preparation: polyetheretherketone fiber filament 21 is selected as the weaving material; S202: Weaving and forming: the inner tube 1 prepared in S1 is positioned on a three-dimensional weaving machine, and the polyetheretherketone fiber filaments 21 are weaved on the outer wall of the inner tube 1 by the three-dimensional weaving machine to form an intermediate braided tube 2; S3: Preparation of outer tube 3, including the following steps: S301: Raw material preparation: Polyetheretherketone heat shrink tube is selected as the material of the outer tube 3; S302: Sleeve connection: coaxially sleeve the polyetheretherketone heat shrink tube outside the middle braided tube 2; S303: heat shrinkage treatment: external heating is used to shrink the polyetheretherketone heat shrinkable tube inward to form an outer layer tube 3 that is closely attached to the outer surface of the middle braided tube 2; S304: Cooling and shaping: ensuring that the outer tube 3 after heat shrinkage is completely cooled and shaped; S4: Formation of the vacuum insulation cavity a, comprising the following steps: S401: vacuum preparation: blocking both ends of the composite conduit, and opening at least one vacuum hole b for vacuuming on the blocked composite conduit; S402: vacuum treatment: using a vacuum device to extract the air between the inner tube 1 and the outer tube 3 through the reserved air extraction hole b, and supporting the gap between the inner tube 1 and the outer tube 3 through the middle braided tube 2, so that a vacuum heat insulation cavity a is formed between the inner tube 1 and the outer tube 3; S403: Sealing process: After the vacuuming is completed, the vacuum hole b on the composite conduit is sealed to ensure that the composite conduit remains in a vacuum state; S404: Vacuum testing: Performing a vacuum pressure test on the vacuum insulation cavity a of the composite conduit through a pressure testing device to ensure that the vacuum insulation cavity a of the composite conduit can maintain a vacuum state within a predetermined time, so as to ensure that the vacuum insulation cavity a has no leakage; S5: Post-processing: grinding and coating the outer surface of the composite catheter.

[0032] In the preparation method of the above-mentioned vacuum insulated polyetheretherketone composite conduit, the mechanical grinding treatment adopted in step S104 is mainly suitable for the situation that small area manual grinding is required. It is necessary to clean the oil stains on the surface of the inner tube 1 first, and then use a handheld grinder equipped with a grinding wheel or sandpaper disc with different particle sizes to grind the outer wall of the inner tube 1. After that, an electric polishing machine can be used to perform a more fine grinding treatment on the outer wall of the inner tube 1; in this embodiment, the mesh range of the sandpaper or grinding wheel is set between 60-600 mesh, and the rotation speed of the grinder or polisher is set to 2500-30000 rpm. Medium and high speeds are suitable for rough grinding, and low speeds are suitable for fine grinding. The outer surface of the inner tube 1 is ground by first rough grinding and then fine grinding; the chemical reagent treatment used in step S104 can be selected from one of the pickling or alkali washing methods for weaving, wherein the pickling treatment often uses hydrochloric acid or sulfuric acid with a concentration of 5% to remove impurities on the surface of the inner tube 1, and the alkali washing treatment often uses an alkaline solution containing sodium hydroxide with a concentration of 5% to remove grease on the surface of the inner tube 1. After the pickling or alkali washing is completed, the outer surface of the inner tube needs to be enhanced, and a silane coupling agent is often used to enhance the outer surface of the inner tube 1 and the outer surface of the inner tube 1. The bonding strength between the middle braided tube 2, wherein the surface chemical treatment time of the inner tube 1 by acid washing or alkali washing is controlled between 5-120 minutes, and the inner tube 1 needs to be thoroughly rinsed with clean water after the surface chemical treatment is completed, and further cleaned with deionized water, and finally the water stains on the surface of the inner tube 1 are dried naturally or blown dry with compressed air; the diameter of the polyetheretherketone fiber filament 21 in step S201 is set between 50-200 microns, and in this embodiment, the diameter of the polyetheretherketone fiber filament 21 is set to 100 microns, and the smaller diameter of the polyetheretherketone fiber filament 21 can improve the bonding strength between the middle braided tube 2 The flexibility of the intermediate braided tube 2 can be increased by a larger diameter of the polyetheretherketone fiber filament 21, so the diameter of the polyetheretherketone fiber filament 21 is set to 100 microns, which can ensure that the intermediate braided tube 2 has good flexibility and a certain structural strength; the braiding density of the polyetheretherketone fiber filament 21 of the intermediate braided tube 2 in step S202 is set between 5 and 20 strands / cm. In this embodiment, the braiding density of the polyetheretherketone fiber filament 21 of the intermediate braided tube 2 is set to 15 strands / cm, so that the intermediate braided tube 2 has both high compressive strength and structural strength, and can also have a certain flexibility;In addition, the three-dimensional braiding machine of the intermediate braided tube 2 in step S202 adopts one of the plain weave, twill weave or satin weave methods for weaving. Different weaving patterns will affect the flexibility and compression resistance of the braided layer. Among them, the intermediate braided tube 2 formed by plain weaving has better flexibility, while the intermediate braided tube 2 formed by twill weaving and satin weaving has higher strength and compression resistance. Medical personnel can choose the composite catheter prepared by the corresponding weaving method according to the actual scene needs. In this embodiment, the intermediate braided tube 2 adopts the twill weaving method. The inner tube 1 is braided outside, and the braiding angle is set to 45°, so that the braided intermediate braided tube 2 has good lateral flexibility; the blocking treatment in step S401 and the sealing treatment in step S403 are both adopted by heat melting or glue bonding at both ends of the inner tube 1 and the outer tube 3, and the exhaust hole b is opened on the corresponding heat melting surface or glue bonding surface 5. When the composite conduit is vacuum treated, the ends of the inner tube 1 and the outer tube 3 are first sealed by heat melting or glue bonding, and then the exhaust hole b is opened on the heat melting surface or glue bonding surface 5. The pore b is then vacuumed by a vacuum pumping device to form a vacuum insulation cavity a. When the vacuuming is completed, the pore b is sealed again by hot welding or glue bonding to achieve vacuum sealing of the vacuum insulation cavity a. In step S404, the pressure holding time of the vacuum pressure holding test is controlled between 20 and 120 minutes. In step S5, the outer surface of the composite catheter is mechanically polished, and then a hydrophilic coating is applied to the polished outer wall of the composite catheter. In addition, after step S5, the prepared composite catheter needs to be tested for performance, mainly for two major performance tests, including flexibility test and pressure resistance test. The flexibility test uses a three-point bending test device to perform a bending fatigue test to simulate the bending of the catheter in a complex anatomical structure. The results show that the composite catheter can still maintain good flexibility after multiple bending cycles without obvious fracture or damage. The pressure resistance test uses a bursting pressure test device to perform a compression load test to simulate the performance of the catheter under internal and external pressure. The results show that when the composite catheter is subjected to water pressure shock, the test shows that the composite catheter prepared by the present invention has a bursting pressure greater than the existing composite catheters on the market. ; Specific embodiment 2 like Figure 3As shown, the difference between this embodiment and the specific embodiment 1 lies in the opening position of the exhaust hole b of the vacuum insulation polyetheretherketone composite conduit and the sealing treatment method adopted in step S03 of the preparation method; the sealing treatment in step S401 of this embodiment adopts the method of heat welding or gluing at both ends of the inner tube 1 and the outer tube 3, and the exhaust hole b is opened on the outer wall of the outer tube 3. The sealing treatment in step S403 adopts a layer of sealing tube 4 that is aligned with the position of the exhaust hole b outside the outer tube 3. The sealing tube 4 is made of polyetheretherketone heat shrink tube cut and made by The sealing tube 4 is heated to shrink it and wrap around the outer tube 3, and the exhaust hole b is sealed. When the composite conduit is vacuum-treated, the ends of the inner tube 1 and the outer tube 3 are first sealed by heat melting or gluing, and then the exhaust hole b is opened on the outer wall of the outer tube 3. After that, a vacuum is drawn using a vacuum pumping device to form a vacuum insulation cavity a. After the vacuuming is completed, a layer of polyetheretherketone heat shrinkable tube is sheathed on the outside of the outer tube 3, and the outermost layer of polyetheretherketone heat shrinkable tube is heat-shrunk and wrapped around the outer tube 3 by heating, thereby achieving vacuum sealing of the vacuum insulation cavity a.

[0034] The other structures and methods of this embodiment are the same as those of the first embodiment and will not be described in detail here.

[0035] The above description is only a preferred embodiment of the present invention, so all equivalent changes or modifications made according to the structure, characteristics and principles described in the scope of the patent application of the present invention are included in the scope of the patent application of the present invention.

Claims

1. A vacuum insulated polyetheretherketone composite conduit, Features: The invention comprises an inner tube (1), an outer tube (3) and an intermediate braided tube (2) arranged between the inner tube (1) and the outer tube (3); the materials of the inner tube (1), the intermediate braided tube (2) and the outer tube (3) are all set to polyetheretherketone; the outer tube (3) is tightly wrapped around the outside of the intermediate braided tube (2); the outer tube (3) and the inner tube (1) are sealed at both ends; and a vacuum heat-insulating cavity a is formed between the outer tube (3) and the inner tube (1).

2. A vacuum insulated polyetheretherketone composite conduit according to claim 1, Features: The outer layer tube (3) is configured as a polyetheretherketone heat shrink tube, and the outer layer tube (3) is tightly coated on the outer wall of the middle braided tube (2) through a heat shrink process.

3. The vacuum insulated polyetheretherketone composite conduit according to claim 1, Features: The intermediate braided tube (2) is formed by three-dimensionally braiding a plurality of polyetheretherketone fiber filaments (21) outside the inner tube (1), and hollow mesh holes 2a for air flow are formed between adjacent polyetheretherketone fiber filaments (21).

4. The vacuum insulated polyetheretherketone composite conduit according to claim 1, Features: The number of coaxial braiding layers of the intermediate braided tube (2) is set to at least one layer.

5. A method for preparing the vacuum insulated polyetheretherketone composite conduit according to any one of claims 1 to 4, It is characterized in that The following steps are involved: S1: Preparation of the inner layer tube (1), comprising the following steps: S101: Raw material preparation: Polyetheretherketone granules are selected as raw materials; S102: extrusion molding: heating the polyetheretherketone pellets to a melting point of 334° C. or higher, and extruding them through an extruder to form a hollow inner tube (1); S103: Cooling and shaping: cooling and shaping the inner layer tube (1) after extrusion in a cooling water tank; S104: Surface treatment: mechanically grinding the outer wall of the inner tube (1) or treating the outer surface with a chemical agent to enhance the bonding force between the outer surface of the inner tube (1) and the middle braided tube (2); S2: Preparation of the intermediate braided tube (2), comprising the following steps: S201: Raw material preparation: polyetheretherketone fiber (21) is selected as the braiding material; S202: Weaving and forming: the inner tube (1) prepared in S1 is positioned on a three-dimensional weaving machine, and the polyetheretherketone fiber filaments (21) are weaved on the outer wall of the inner tube (1) by the three-dimensional weaving machine to form an intermediate braided tube (2); S3: Preparation of the outer tube (3), comprising the following steps: S301: Raw material preparation: Polyetheretherketone heat shrink tube is selected as the material of the outer tube (3); S302: Sleeve connection: coaxially sleeve the polyetheretherketone heat shrink tube outside the middle braided tube (2); S303: heat shrinkage treatment: externally heating the polyetheretherketone heat shrinkable tube to shrink inwardly, thereby forming an outer layer tube (3) that is closely fitted to the outer surface of the middle braided tube (2); S304: Cooling and shaping: ensuring that the outer tube (3) after heat shrinkage is completely cooled and shaped; S4: Formation of the vacuum insulation cavity a, comprising the following steps: S401: vacuum preparation: blocking both ends of the composite conduit, and opening at least one vacuum hole b for vacuuming on the blocked composite conduit; S402: vacuum treatment: using a vacuum device to extract the air between the inner tube (1) and the outer tube (3) through the reserved air extraction hole b, and supporting the gap between the inner tube (1) and the outer tube (3) through the intermediate braided tube (2), so that a vacuum heat insulation cavity a is formed between the inner tube (1) and the outer tube (3); S403: Sealing process: After the vacuuming is completed, the vacuum hole b on the composite conduit is sealed to ensure that the composite conduit remains in a vacuum state; S404: Vacuum testing: Performing a vacuum pressure test on the vacuum insulation cavity a of the composite conduit through a pressure testing device to ensure that the vacuum insulation cavity a of the composite conduit can maintain a vacuum state within a predetermined time, so as to ensure that the vacuum insulation cavity a has no leakage; S5: Post-processing: grinding and coating the outer surface of the composite catheter.

6. The method for preparing the vacuum insulated polyetheretherketone composite conduit according to claim 5, Features: The diameter of the polyetheretherketone fiber (21) in step S201 is set between 50-200 microns.

7. The method for preparing the vacuum insulated polyetheretherketone composite conduit according to claim 5, Features: The braiding density of the polyetheretherketone fiber filaments (21) of the intermediate braided tube (2) in step S202 is set between 5 and 20 strands / cm.

8. The method for preparing the vacuum insulated polyetheretherketone composite conduit according to claim 5, Features: The three-dimensional weaving machine of the intermediate braided tube (2) in step S202 weaves in one of the following ways: plain weaving, twill weaving or satin weaving.

9. The method for preparing the vacuum insulated polyetheretherketone composite conduit according to claim 5, Features: The blocking process in step S401 and the sealing process in step S403 are both performed by heat-melting or gluing the two ends of the inner tube (1) and the outer tube (3), and the air extraction hole b is opened on the corresponding heat-melting surface or glue bonding surface (5).

10. The method for preparing the vacuum insulated polyetheretherketone composite conduit according to claim 5, Features: The blocking treatment in step S401 is performed by heat-melting or gluing the two ends of the inner tube (1) and the outer tube (3), and the exhaust hole b is opened on the outer wall of the outer tube (3). The sealing treatment in step S403 is performed by sleeve-connecting a layer of sealing tube (4) on the outside of the outer tube (3) in alignment with the position of the exhaust hole b. The sealing tube (4) is made by cutting and forming a polyetheretherketone heat shrink tube. The sealing tube (4) is heated to shrink and wrap around the outer tube (3), and the exhaust hole b is blocked.

Citation Information

Patent Citations

  • Implant delivery device

    CN103037776A

  • IVC filter retrieval systems with interposed support members

    CN112220585A

  • Multi-layer composite polyether-ether-ketone pipe

    CN113775857A

  • Balloon microcatheter and preparation method thereof

    CN114288528A

  • Stent delivery catheter and preparation method thereof

    CN116672140A

Cited By

  • PEEK medical composite catheter with developing mark and preparation method of PEEK medical composite catheter

    CN119564997A

  • PEEK Medical Composite Catheter with Development Markers and Its Preparation Method

    CN119564997B

  • Preparation method of microcatheter with gradually-changed hardness

    CN119607369A

  • Composite catheter with end sealed by porous PET (polyethylene terephthalate) film and end sealing method of composite catheter

    CN119701172A

  • Woven reinforced tearable sheath structure and manufacturing method

    CN119818802A