Supported cobalt-indium catalyst and method for preparing fatty aldehyde through reduction hydrogenation of fatty acid by using supported cobalt-indium catalyst

By using a hydrophobic support-loaded CoIn catalyst under mild conditions, the problems of difficulty in preparing long-chain fatty aldehydes and decreasing catalyst activity in the prior art are solved, and high selectivity and high yield fatty aldehyde production is achieved, which significantly improves the catalyst Stability and reaction rate.

CN119016056APending Publication Date: 2024-11-26CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411111062.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently and economically prepare long-chain fatty aldehydes, and the activity of existing catalysts decreases under high temperature and high pressure conditions, has low yields, and the fatty aldehydes are easily hydrogenated into alcohols, and have low selectivity.

Method used

The hydrophobic support is used to carry bimetallic (CoIn) catalyst, and the hydrophobic support and catalyst are prepared by room temperature stirring, oven drying and calcining of muffle furnaces. It is used to catalyze the hydrodeoxygenation reaction of fatty acids under mild conditions to avoid contact with the catalyst. Improve reaction rate and catalyst stability.

Benefits of technology

A high yield of high selective fatty aldehydes is achieved, and the continued conversion of fatty aldehydes into alcohol is avoided, and the stability and reaction rate of the catalyst are improved, with the yield reaching more than 80.0%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016056A_ABST
    Figure CN119016056A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysts, and discloses a supported cobalt indium catalyst and a method for preparing fatty aldehyde through reduction hydrogenation of fatty acid by using the supported cobalt indium catalyst. The preparation method comprises the following steps: weighing water-soluble indium salt and water-soluble cobalt salt at room temperature, dissolving the water-soluble indium salt and the water-soluble cobalt salt in deionized water to obtain a metal precursor impregnation liquid, carrying out equivalent-volume impregnation on the metal precursor impregnation liquid and a hydrophobic carrier, drying, and calcining to obtain the bimetallic-loaded CoIn catalyst; the CoIn catalyst is used in a reaction for catalyzing fatty acid to convert fatty aldehyde after reduction activity, the fatty acid is subjected to high-selectivity hydrodeoxygenation in a reaction system to generate fatty aldehyde through mutual cooperation of Co and In, and high selectivity and yield can still be obtained in preparation of long-chain fatty aldehyde.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to a reaction in which a carrier-supported bimetallic (CoIn) catalyst is used for reduction and hydrogenation of fatty acids to prepare fatty aldehydes. Background Art

[0002] Long-chain fatty aldehydes exist as free lipids in various organisms, appear as decomposition intermediates, and are rapidly converted into alcohols or carboxylic acids, so aldehydes are rarely detected in mammalian cells. In production and life, long-chain fatty aldehydes are of great significance as odorants for food and beverages. In industrial production, aldehyde compounds are generally prepared by hydroformylation of olefins. Another method for synthesizing fatty aldehydes is the dehydration of fatty alcohols, which is a typical process for producing long-chain aldehydes. Both methods use fossil raw materials, and the reaction conditions are harsh, requiring high temperature and high pressure. Considering the scarcity of fossil raw materials today and the importance of developing green chemistry, there have been reports on the extraction of fatty aldehydes from natural products, but the yield of fatty aldehydes produced by these methods is low. For example, M Palma performed continuous supercritical fluid extraction on white grape seeds, and the fractionated extracted compounds mainly contained fatty acids, fatty aldehydes and sterols, with a fatty aldehyde yield of 10%.

[0003] There are many reports that bimetallic catalysts catalyze the hydrodeoxygenation of fatty acids, such as NiFe, NiCu, NiMo, NiSn, CoFe, and CoRe loaded on zeolites or metal oxides. Fatty aldehydes are intermediate products. Since aldehydes are easily hydrogenated into alcohols, their selectivity is extremely low or even undetectable, and it is impossible to collect aldehydes with high selectivity. Common catalysts will have a decreased catalytic effect as the carbon chain of the substrate fatty acid increases. It is even more difficult to prepare long-chain fatty aldehydes with a high yield.

[0004] In addition, during the process of hydrodeoxygenation of fatty acids (such as hexadecanoic acid) to generate fatty aldehydes (such as hexadecane), oxygen atoms are eventually removed in the form of H2O, and the generated water will be adsorbed on the catalyst surface, destroying the catalyst structure, inhibiting the reaction catalysis, resulting in a decrease in reaction rate and deactivation of the catalyst. If the catalyst is hydrophobic, it can be effectively dispersed in the organic solvent to avoid contact between water molecules and the catalyst, thereby promoting the dispersion of the loaded metal on the carrier, providing more active sites for the hydrodeoxygenation reaction, and improving the deoxygenation rate and stability of the catalyst.

[0005] It is desirable to develop a high-yield fatty aldehyde production process using renewable resources as raw materials and using hydrophobic carrier-supported bimetallic catalysts. The present invention introduces a new process for preparing fatty aldehydes using renewable raw materials and mild reaction conditions. Summary of the invention

[0006] In order to solve the problems in the background technology, the present invention proposes a hydrophobic carrier-supported bimetallic (CoIn) catalyst, which achieves high selectivity in generating fatty aldehydes from fatty acids.

[0007] The specific preparation method of the hydrophobic carrier is as follows:

[0008] Weigh the organosilane reagent, solvent and carrier at room temperature, mix them, stir at room temperature for 2 hours, then continue stirring in a 80°C water bath for 3-5 hours, centrifuge at 5000-7000 rpm for 5 minutes, dry in an oven at 80-120°C, heat from room temperature to 100°C in a muffle furnace at a heating rate of 2°C / min, then heat from 100°C to 450°C at a heating rate of 3°C / min, maintain at 450°C for 4 hours, cool to room temperature and grind to obtain a hydrophobic carrier.

[0009] Further: the organosilane reagent is a mixture of one or more of trimethylchlorosilane, trimethoxysilane, triethylchlorosilane, vinyltrimethoxysilane and hexadecyltrimethoxysilane, which plays a role of hydrophobic modification. Based on cost considerations, trimethylchlorosilane is preferred.

[0010] Furthermore, the solvent is an ethanol solution with a mass fraction of 95%.

[0011] Furthermore, the carrier is titanium dioxide or silicon dioxide, or a mixture of the two.

[0012] Furthermore, the mass ratio of the organic silane hydrophobic agent, the solvent 95% ethanol and the carrier is 0.6:30:1 to 1.2:30:1; preferably, the mass ratio of the hydrophobic agent trimethylchlorosilane, 95% ethanol and the carrier is 1:30:1.

[0013] The specific preparation method of the catalyst is as follows:

[0014] At room temperature, water-soluble indium salt and water-soluble cobalt salt were weighed and dissolved in deionized water to obtain a metal precursor impregnation solution, which was then impregnated with an equal volume of a hydrophobic carrier and placed at room temperature for 12 hours. The solution was then dried in an oven, heated from room temperature to 100°C in a muffle furnace at a heating rate of 2°C / min, and then calcined from 100°C to 450°C at a rate of 3°C / min, maintained at this temperature for 2 to 4 hours, and finally ground to obtain a catalyst.

[0015] The total loading amount of the metal in the metal precursor solution is 6%, and the molar ratio of metal In:Co is 2:1 to 1:6, and more preferably 1:1 to 1:3.

[0016] The purpose of the carrier is mainly to promote the dispersion of the bimetallic active components.

[0017] The calcination temperature of 450°C is the preferred calcination condition. If the temperature is too high, Co will form an alloy with Ti, and oxygen-deficient compounds will be easily generated. The carrier may also be crystallized again, which is not conducive to the activity of the catalyst.

[0018] The obtained catalyst is used in the reaction of catalyzing the conversion of fatty acids into fatty aldehydes. The application method is as follows: weigh the catalyst and put it into a reduction tube, and activate it in a high-temperature reduction furnace at 350-450°C under H2 atmosphere. Reduction procedure: the room temperature is raised to 350-450°C, the heating rate is 2°C / min, and the time at 350-450°C is maintained for 4 hours. The solvent and the substrate are added to the Parr kettle, and the reduced catalyst is quickly poured into the kettle under the protection of hydrogen gas. The reaction lasts for 2 hours in total, and the reaction is collected every 15 minutes. The product liquid is centrifuged and filtered, and then analyzed by gas chromatography.

[0019] The mass ratio of catalyst: substrate: solvent is 0.3-0.5:1:89.6; the solvent is decahydronaphthalene, the reaction temperature is 240-280°C; the pressure is 0.6-2MPa; and the rotation speed is 300-700rpm.

[0020] CH3(CH2) n COOH→CH3(CH2) n COH, wherein n is 4-17.

[0021] Compared with the prior art, the advantages of the present invention are:

[0022] Hydrophobic catalysts can be effectively dispersed in organic solvents to avoid contact between trace water molecules generated by the reaction and the catalyst, providing more active sites for the hydrodeoxygenation reaction, improving the deoxygenation rate and catalyst stability. Fatty aldehydes can no longer be converted under these reaction conditions, and In can inhibit the further hydrogenation of fatty aldehydes into fatty alcohols. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a graph showing the conversion rate of hexadecanoic acid and the yield of hexadecanoic acid aldehyde after continuous reaction for 2 hours in Example 1.

[0024] Figure 2 This is a graph showing the conversion rate of hexadecanoic acid and the yield of hexadecanoic aldehyde after continuous reaction for 2 hours in Comparative Example 3.

[0025] Figure 3 This is the XRD diffraction pattern of the hydrophobic CoIn@TiO2 catalyst obtained in Example 1. The atomic ratio of CoIn is 3:1. DETAILED DESCRIPTION

[0026] The present invention is further described in detail below in conjunction with the examples, but the present invention is not limited to the following examples. The raw materials and equipment used can all be purchased from the market. The methods in the following examples, unless otherwise specified, are conventional methods in the art. Titanium dioxide was purchased from Xuancheng Jingrui New Materials (VK-T25); silicon dioxide was purchased from Qingdao Shuoyuan Silicone Technology Co., Ltd.

[0027] Example 1

[0028] (1) Preparation of hydrophobic TiO2 carrier: 5 g trimethylsilyl chloride, 150 g 95% ethanol and 5 g TiO2 carrier were weighed at room temperature and mixed. The mixture was stirred at room temperature for 2 h, stirred in an 80°C water bath for 4 h, centrifuged and dried in a 60°C oven overnight. The mixture was heated from room temperature to 100°C in a muffle furnace at a heating rate of 2°C / min, and then the calcination temperature was increased from 100°C to 450°C at a rate of 3°C / min for 4 h. The hydrophobic carrier was then ground.

[0029] (2) CoIn catalyst loaded on hydrophobic TiO2 carrier: 0.538 g of cobalt nitrate hexahydrate and 0.252 g of indium nitrate hexahydrate were weighed and dissolved in 1.5 g of deionized water at room temperature to obtain a metal precursor impregnation solution, wherein the molar ratio of Co:In=3:1. 3.0 g of carrier TiO2 was weighed and impregnated with equal volumes. After drying at room temperature overnight and in an oven at 100°C for 6 h, the temperature was raised from room temperature to 100°C in a muffle furnace at a heating rate of 2°C / min, and then the calcination temperature was raised from 100°C to 450°C at a rate of 3°C / min for 2 h. The catalyst was ground to obtain the catalyst.

[0030] (3) Hydrodeoxygenation of hexadecanoic acid to produce hexadecanoic acid: Weigh 0.3 g of catalyst into a reduction tube and activate it in a high-temperature reduction furnace at 450°C under H2 atmosphere. The reduction procedure is to increase the temperature from room temperature to 450°C at a heating rate of 2°C / min and maintain it at this temperature for 4 hours. Add 100 mL of decahydronaphthalene and 1 g of hexadecanoic acid to the Parr kettle. After the temperature of the reduction tube drops to room temperature, gas protection is performed. The catalyst is quickly introduced into the kettle under H2 atmosphere. The Parr kettle speed is 500 rpm. When the temperature rises to 260°C, 1 MPa of H2 is filled. The reaction lasts for 2 hours. The collected product liquid is centrifuged and filtered, and then analyzed by gas chromatography. After continuous operation for 2 hours, the product yield is 80.0%.

[0031] The XRD pattern of the catalyst after reduction passivation used in Example 1 ( Figure 3), where the characteristic peaks at 2θ=27.45°, 36.05°, 39.22°, 41.23°, 44.81°, 54.32°, 54.30°, 62.74°, 64.04°, 69.25° and 69.78° are consistent with the structure of TiO2, indicating that the loading of metals does not change the structure of TiO2. No obvious characteristic peaks were found for Co and In, indicating that Co and In are highly dispersed in the catalyst.

[0032] Example 2

[0033] The reaction condition of the parr reactor in step (3) of Example 1 was changed to charging 0.6 MPa H2. Other operations were the same as in Example 1. The reaction lasted for 2 hours. The collected product liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the product yield was 77.9%.

[0034] Example 3

[0035] The reaction condition of the parr reactor in step (3) of Example 1 was changed to charging with 2MPa H2. Other operations were the same as in Example 1. The reaction lasted for 2 hours. The collected product liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the product yield was 72.9%.

[0036] Example 4

[0037] The 0.538 g of cobalt nitrate hexahydrate and 0.252 g of indium nitrate hexahydrate in step (2) of Example 1 were replaced with 0.450 g of cobalt nitrate hexahydrate and 0.316 g of indium nitrate hexahydrate, wherein the molar ratio of Co:In=2:1, and the other operations were the same as in Example 1. The reaction lasted for 2 hours, and the collected product liquid was centrifuged, filtered, and then analyzed by gas chromatography. After continuous operation for 2 hours, the product yield was 76.5%.

[0038] Example 5

[0039] The 0.538 g of cobalt nitrate hexahydrate and 0.252 g of indium nitrate hexahydrate in step (2) of Example 1 were replaced with 0.302 g of cobalt nitrate hexahydrate and 0.424 g of indium nitrate hexahydrate, wherein the molar ratio of Co:In=1:1. The other operations were the same as in Example 1. The reaction lasted for 2 hours, and the collected product liquid was centrifuged, filtered, and analyzed by gas chromatography. After continuous operation for 2 hours, the product yield was 75.1%.

[0040] Example 6

[0041] The 0.538 g of cobalt nitrate hexahydrate and 0.252 g of indium nitrate hexahydrate in step (2) of Example 1 were replaced with 0.182 g of cobalt nitrate hexahydrate and 0.510 g of indium nitrate hexahydrate, wherein the molar ratio of Co:In=1:2. The other operations were the same as in Example 1. The reaction lasted for 2 hours, and the collected liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the product yield was 72.4%.

[0042] Example 7

[0043] The rotation speed of the parr kettle in step (3) of Example 1 was changed from 500 rpm to 300 rpm. Other operations were the same as in Example 1. The reaction lasted for 2 hours. The collected liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the product yield was 75.4%.

[0044] Example 8

[0045] The rotation speed of the parr kettle in step (3) of Example 1 was changed from 500 rpm to 700 rpm. Other operations were the same as those in Example 1. The reaction lasted for 2 hours. The collected liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the product yield was 70.6%.

[0046] Example 9

[0047] The reaction temperature in step (3) of Example 1 was changed from 260°C to 240°C. Other operations were the same as in Example 1. The reaction lasted for 2 hours. The collected liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the product yield was 68.8%.

[0048] Example 10

[0049] The reaction temperature in step (3) of Example 1 was changed from 260°C to 280°C. Other operations were the same as in Example 1. The reaction lasted for 2 hours. The collected liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the product yield was 72.0%.

[0050] Embodiment 11

[0051] The calcination temperature of 450°C in step (2) of Example 1 was changed to 350°C, and the temperature was raised from room temperature to 100°C at a heating rate of 2°C / min, and then the calcination temperature was raised from 100°C to 350°C at a rate of 3°C / min for 4 hours. Other operations were the same as in Example 1. The reaction lasted for 2 hours, and the collected product liquid was analyzed by gas chromatography after centrifugation and filtration. After continuous operation for 2 hours, the product yield was 75.0%.

[0052] Example 12

[0053] The TiO2 carrier in step (1) of Example 1 was replaced by SiO2, and the other operations were the same as those of Example 1. The reaction lasted for 2 hours, and the collected product liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the yield of hexadecanal product was 78.6%.

[0054] Example 13

[0055] The substrate hexadecanoic acid in step (3) of Example 1 was replaced by lauric acid, and the other operations were the same as in Example 1. The reaction lasted for 2 hours, and the collected product liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the yield of lauric aldehyde product was 84.8%.

[0056] Embodiment 14

[0057] The substrate hexadecanoic acid in step (3) of Example 1 was replaced with stearic acid, and the other operations were the same as in Example 1. The reaction lasted for 2 hours, and the collected product liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the yield of octadecanal product was 77.2%.

[0058] Embodiment 15

[0059] The substrate hexadecanoic acid in step (3) of Example 1 was replaced with hexanoic acid, and the other operations were the same as in Example 1. The reaction lasted for 2 hours, and the collected product liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the yield of hexanal product was 92.5%.

[0060] Example 16

[0061] The substrate hexadecanoic acid in step (3) of Example 1 was replaced by decanic acid, and the other operations were the same as in Example 1. The reaction lasted for 2 hours, and the collected product liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 2 hours, the yield of decanal product was 90.8%.

[0062] Embodiment 17

[0063] The reaction condition of the parr reactor in step (3) of Example 1 was changed to charging 0.6 MPa H2. Other operations were the same as in Example 1. The reaction lasted for 8 hours. The collected product liquid was centrifuged and filtered and then analyzed by gas chromatography. After continuous operation for 8 hours, the product yield was 69.4%.

[0064] Comparative Example 1

[0065] Compared with Example 1, the TiO2 carrier was not hydrophobically modified, and the catalyst was directly loaded on the TiO2 carrier at a molar ratio of Co:In=3:1. The other operations were the same as in Example 1: the catalyst reaction lasted for a total of 2 hours, and the collected product liquid was analyzed by gas chromatography after centrifugation and filtration. After continuous operation for 2 hours, the product yield was 37.6%.

[0066] Comparative Example 2

[0067] Compared with Example 12, the SiO2 carrier was not hydrophobically modified, and the catalyst was directly loaded on the SiO2 carrier with a molar ratio of Co:In=3:1. The other operations were the same as Example 12: the catalyst reaction lasted for a total of 2 hours, and the collected product liquid was analyzed by gas chromatography after centrifugation and filtration. After continuous operation for 2 hours, the product yield was 34.1%.

[0068] In the above comparative example 1 and example 2, we respectively selected TiO2 and SiO2 which had not been treated with hydrophobicity as carriers for comparison. The reaction rate on the catalyst after impregnation with CoIn was significantly reduced, and the amount of generated aldehyde was also reduced.

[0069] Comparative Example 3

[0070] Compared with Example 1, only In is loaded, and the amount of loaded In is the same as the total amount of CoIn. A single-loaded In catalyst on a hydrophobic TiO2 carrier is prepared.

[0071] The reaction results of using hydrophobic TiO2 as a carrier and loading In alone were as follows: the reaction lasted for 2 hours, and the collected product liquid was analyzed by gas chromatography after centrifugation and filtration. After continuous operation for 2 hours, the yield of hexadecanal product was 14.6%.

[0072] Comparative Example 4

[0073] Compared with Example 1, only Co is loaded, and the amount of In loaded is the same as the total amount of CoIn. A hydrophobic TiO2 carrier single-loaded Co catalyst is prepared.

[0074] The reaction results of using hydrophobic TiO2 as a carrier and loading Co alone were as follows: the reaction lasted for 2 hours, and the collected product liquid was analyzed by gas chromatography after centrifugation and filtration. After continuous operation for 2 hours, the yield of hexadecanal product was 39.2%.

[0075] Comparative Example 5

[0076] Compared with Example 1, an equal molar amount of In was replaced by Ga, and other operations were the same. A hydrophobic TiO2 carrier-supported CoGa catalyst was prepared.

[0077] The reaction results of CoCa loaded with hydrophobic TiO2 as the carrier: the reaction lasted for 2 hours. The collected product liquid was analyzed by gas chromatography after centrifugation and filtration. After continuous operation for 2 hours, the product yield was 0%.

[0078] In the above comparative example 3, we selected CoGa, which can easily generate hexadecanol on the catalyst of CoGa supported on hydrophobic TiO2.

[0079] Although the embodiments of the present invention have been described in detail, it should be understood that the various changes, substitutions, and alterations could be made hereto without departing from the spirit and scope of the invention.

Claims

1. A supported bimetallic cobalt-indium catalyst for the reduction and hydrogenation of fatty acids to produce fatty aldehydes, characterized in that: The preparation method comprises the following steps: mixing indium salt and cobalt salt to prepare metal precursor impregnation solution, impregnating the metal precursor impregnation solution onto a carrier, and drying, calcining and grinding to obtain a supported bimetallic cobalt indium catalyst.

2. The supported bimetallic cobalt-indium catalyst for the reduction and hydrogenation of fatty acids to produce fatty aldehydes according to claim 1, characterized in that: The carrier is titanium dioxide or silicon dioxide or a mixture of the two.

3. The supported bimetallic cobalt-indium catalyst for the reduction and hydrogenation of fatty acids to produce fatty aldehydes according to claim 1, characterized in that: The carrier is a hydrophobically modified carrier; the hydrophobic modification method is: weighing an organic silane reagent, a solvent and a carrier at room temperature, mixing them, stirring at room temperature, stirring in a water bath, centrifuging, drying in an oven, calcining in a muffle furnace, and grinding to obtain a hydrophobic carrier.

4. The supported bimetallic cobalt-indium catalyst for the reduction and hydrogenation of fatty acids to produce fatty aldehydes according to claim 3, characterized in that: The organosilane reagent is a mixture of one or more of trimethylchlorosilane, trimethoxysilane, triethylchlorosilane, vinyltrimethoxysilane and hexadecyltrimethoxysilane; the solvent is an ethanol solution with a mass fraction of 95%; the mass ratio of the organosilane reagent, the solvent and the carrier is 0.6:30:1 to 1.2:30:

1.

5. The supported bimetallic cobalt-indium catalyst for the reduction and hydrogenation of fatty acids to produce fatty aldehydes according to claim 1, characterized in that: The molar ratio of In:Co is 2:1 to 1:

6.

6. The supported bimetallic cobalt-indium catalyst for the reduction and hydrogenation of fatty acids to produce fatty aldehydes according to claim 1, characterized in that: The calcination conditions are as follows: the temperature is increased from room temperature to 100°C at a heating rate of 2°C / min, and then the calcination temperature is increased from 100°C to 450°C at a heating rate of 3°C / min, and maintained at this temperature for 2 to 4 hours.

7. A method for preparing fatty aldehydes by reducing and hydrogenating fatty acids using the supported bimetallic cobalt indium catalyst according to any one of claims 1 to 6, characterized in that: The loaded bimetallic CoIn catalyst is reduced, a solvent and a fatty acid are added into a reactor, and the reduced catalyst is quickly poured into the reactor under a H2 atmosphere to react to obtain a fatty aldehyde.

8. The method for preparing fatty aldehydes by reducing and hydrogenating fatty acids using the supported bimetallic cobalt indium catalyst according to claim 7, characterized in that: The solvent is decahydronaphthalene, the reaction temperature is 240-280°C; the reaction pressure is 0.6-2MPa; the reaction speed is 300-700rpm, and the reaction time is 2h.

9. The method for preparing fatty aldehydes by reducing and hydrogenating fatty acids using the supported bimetallic cobalt indium catalyst according to claim 7, characterized in that: The reaction formula is: CH3(CH2) n COOH→CH3(CH2) n COH, wherein n is 4-17.

10. The method for preparing fatty aldehydes by reducing and hydrogenating fatty acids using the supported bimetallic cobalt indium catalyst according to claim 7, characterized in that: Catalyst: fatty acid mass ratio = 0.3-0.5:1.