Catalyst for producing acetonitrile as well as preparation method and application of catalyst
By using catalysts composed of transition metal oxides and non-metal oxides, the corrosion and cost problems of the existing acetonitrile production methods are solved, efficient production and high yield of acetonitrile are achieved, and the reaction conditions are mild, avoiding equipment corrosion .
Patent Information
- Application Number
- CN202310590551.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
The existing acetonitrile production methods have problems such as strong corrosiveness, high cost, slow reaction rate and low conversion rate, and lack safe and effective processes for industrial applications.
A catalyst composed of transition metal oxide and non-metal oxide is prepared by impregnation and calcination methods, and is applied to the reaction of acetate and ammonia to achieve efficient production of acetonitrile.
The high yield of acetonitrile, mild reaction conditions, non-corrosive equipment, and simple preparation method and low cost.
Abstract
Description
Technical Field
[0001] The present application relates to a catalyst for producing acetonitrile and a preparation method and application thereof, belonging to the new technical field of catalyst and chemical production and manufacturing. Background Art
[0002] Acetonitrile is a widely used solvent and an important organic intermediate. Currently, the main production method of acetonitrile is as a byproduct in the production of acrylonitrile. Therefore, its output is limited by the production of acrylonitrile. In recent years, other process routes for acetonitrile production have been studied and developed. For example, ethanol amination method, acetic acid amination method, etc. These methods have the disadvantages of strong corrosiveness and high cost, and have not yet been industrially applied.
[0003] Therefore, based on the current technological status, it is still necessary to develop new acetonitrile production methods and catalysts so that they have the characteristics of non-corrosiveness, safe process operating conditions, fast reaction rate, high reaction conversion rate and atomic utilization rate, and stable reaction. Summary of the invention
[0004] According to a first aspect of the present application, a catalyst for producing acetonitrile is provided.
[0005] A catalyst for producing acetonitrile, the catalyst comprising a transition metal oxide, a non-metal oxide, and a carrier;
[0006] The content of the transition metal oxide in the catalyst is 0.1-5wt%;
[0007] The content of the non-metallic oxide in the catalyst is 1-30 wt %.
[0008] Optionally, the content of the transition metal oxide in the catalyst is independently selected from 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2.0wt%, 2.2wt%, 2.4wt%, 2.6wt%, 2.8wt%, 3.0wt%, 3.2wt%, 3.4wt%, 3.6wt%, 3.8wt%, 4.0wt%, 4.2wt%, 4.4wt%, 4.6wt%, 4.8wt%, 5.0wt%, any value or any range value between two of them.
[0009] Optionally, the content of the non-metallic oxide in the catalyst is independently selected from any value among 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt%, 30wt% or any range value between two of them.
[0010] Optionally, the content of the transition metal oxide in the catalyst is 1-4 wt %.
[0011] Optionally, the content of the transition metal oxide in the catalyst is independently selected from any value among 1.0wt%, 1.2wt%, 1.4wt%, 1.6wt%, 1.8wt%, 2.0wt%, 2.2wt%, 2.4wt%, 2.6wt%, 2.8wt%, 3.0wt%, 3.2wt%, 3.4wt%, 3.6wt%, 3.8wt%, 4.0wt% or any range value between two of them.
[0012] Optionally, the content of the non-metallic oxide in the catalyst is 5-15 wt %.
[0013] Optionally, the content of the non-metallic oxide in the catalyst is independently selected from any value among 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt% or any range value between two of them.
[0014] Optionally, the transition metal oxide is selected from at least one of oxides of Ti, Mn, Fe, Cu, Mo, and W.
[0015] Optionally, the non-metallic oxide is selected from at least one of oxides of B, P, and Se.
[0016] Optionally, the carrier is selected from at least one of alumina, silica, zirconia and kaolin.
[0017] The carrier is a formed carrier.
[0018] The molding method is a conventional molding method in the art.
[0019] According to a second aspect of the present application, a method for preparing a catalyst for producing acetonitrile is provided, and the preparation method is simple and low in cost.
[0020] The method for preparing the catalyst described above comprises the following steps:
[0021] S1, impregnating an aqueous solution containing a soluble metal salt on a carrier, drying I and then calcining I to obtain a catalyst precursor;
[0022] S2. Impregnating the catalyst precursor with an aqueous solution containing a soluble non-metallic compound, drying II and then calcining II to obtain the catalyst.
[0023] Optionally, the soluble metal salt is selected from at least one of TiCl4, manganese nitrate, manganese acetate, ferric nitrate, ferric sulfate, ferric chloride, copper nitrate, ammonium molybdate, and ammonium tungstate.
[0024] Optionally, the soluble non-metallic compound is selected from at least one of boric acid, phosphoric acid and selenium dioxide.
[0025] Optionally, in step S1, the conditions for drying I are as follows:
[0026] The temperature is 100-120℃;
[0027] The time is 12-24h.
[0028] Optionally, the temperature is independently selected from any value among 100°C, 105°C, 110°C, 115°C, 120°C, or any range therebetween.
[0029] Optionally, the time is independently selected from any value of 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, or a range between any two of them.
[0030] Optionally, in step S1, the conditions for roasting I are as follows:
[0031] Temperature is 300-600℃;
[0032] The time is 3-8h.
[0033] Optionally, the temperature is independently selected from any value of 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, or any range therebetween.
[0034] Optionally, the time is independently selected from any value among 3h, 4h, 5h, 6h, 7h, 8h, or any range between two of them.
[0035] Optionally, in step S2, the conditions for drying II are as follows:
[0036] The temperature is 100-120℃;
[0037] The time is 12-24h.
[0038] Optionally, the temperature is independently selected from any value among 100°C, 105°C, 110°C, 115°C, 120°C, or any range therebetween.
[0039] Optionally, the time is independently selected from any value of 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, or a range between any two of them.
[0040] Optionally, in step S2, the conditions for roasting II are as follows:
[0041] Temperature is 300-600℃;
[0042] The time is 3-8h.
[0043] Optionally, the temperature is independently selected from any value of 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, or any range therebetween.
[0044] Optionally, the time is independently selected from any value among 3h, 4h, 5h, 6h, 7h, 8h, or any range between two of them.
[0045] According to the third aspect of the present application, an application of a catalyst for producing acetonitrile is provided. The catalyst is applied to the process of reacting acetate with ammonia to produce acetonitrile, with mild reaction conditions, high acetonitrile yield, and no corrosion to equipment.
[0046] The catalyst described above and / or the catalyst obtained by the preparation method described above is used for the reaction of acetate and ammonia to generate acetonitrile.
[0047] Optionally, the molar ratio of the ammonia gas to the acetate is 1-40:1.
[0048] Optionally, the molar ratio of the ammonia to the acetate is independently selected from any value in 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, 21:1, 22:1, 23:1, 24:1, 25:1, 26:1, 27:1, 28:1, 29:1, 30:1, 31:1, 32:1, 33:1, 34:1, 35:1, 36:1, 37:1, 38:1, 39:1, 40:1 or any range between two of them.
[0049] Optionally, the mass space velocity of the acetate is 0.1-8.0h -1 .
[0050] Optionally, the mass space velocity of the acetate is independently selected from 0.1h -1 、0.2h -1 、0.3h -1 、0.4h -1 , 0.5h -1 、0.6h -1 、0.7h -1 , 0.8h -1 , 0.9h -1 , 1h -1 , 2h -1 , 3h -1 , 4h -1 , 5h -1 , 6h -1 , 7h -1 , 8h -1 Any value in or any range between them.
[0051] Optionally, the reaction conditions are as follows:
[0052] The temperature is 250-500℃.
[0053] Optionally, the temperature is independently selected from any value of 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 350°C, 400°C, 450°C, 500°C, or any range therebetween.
[0054] Optionally, the reaction pressure is 0.1-0.5 MPa.
[0055] Optionally, the reaction pressure is independently selected from any value among 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, or any range between the two.
[0056] Optionally, the reaction is carried out in a reactor selected from at least one of a fixed bed reactor, a tank reactor, a moving bed and a fluidized bed.
[0057] The beneficial effects of this application include:
[0058] 1) The present application provides a catalyst for producing acetonitrile, which is used in the process of reacting acetate with ammonia to generate acetonitrile. The reaction conditions are mild, the acetonitrile yield is high, and it is non-corrosive to equipment.
[0059] 2) The present application provides a method for preparing a catalyst for producing acetonitrile, which is simple and low-cost. DETAILED DESCRIPTION
[0060] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0061] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0062] Unless otherwise specified, conventional test methods or test methods recommended by the instrument shall be used.
[0063] In the examples of this application, the conversion rate and selectivity are calculated as follows:
[0064] Conversion rate of methyl acetate = (1-the number of moles of methyl acetate in the product / the number of moles of methyl acetate in the raw material) * 100%;
[0065] Selectivity of acetonitrile = ((the number of moles of acetonitrile in the product / (the number of moles of methyl acetate in the raw material-the number of moles of methyl acetate in the product))*100%.
[0066] Example 1
[0067] 2.4 g of manganese nitrate was dissolved in water and impregnated on 79 g of a formed silicon oxide carrier. After impregnation, it was dried at 120° C. for 12 hours and then calcined at 450° C. for 3 hours to obtain a catalyst precursor. 27.6 g of phosphoric acid was dissolved in water and impregnated on the above catalyst precursor. It was dried at 120° C. for 12 hours and then calcined at 450° C. for 4 hours to obtain a catalyst A, wherein the transition metal oxide and non-metal oxide of the catalyst A were 1% manganese dioxide and 20% phosphorus pentoxide, respectively.
[0068] 10 g of catalyst A was loaded into a fixed bed reactor, and the catalyst temperature was raised to 320°C. Ammonia was introduced into the reactor. Methyl acetate was introduced into the reactor at a mass space velocity of 1.0 h -1 The molar ratio of ammonia to methyl acetate was 20:1, and the reaction pressure was 0.3 MPa. The products after the reaction were collected and analyzed, and the conversion rate of methyl acetate was 98.5%, and the selectivity of acetonitrile in the amination products was 98.1wt%.
[0069] Example 2
[0070] 4.7g of titanium tetrachloride was dissolved in water and impregnated on 93g of a formed zirconium oxide carrier. After impregnation, it was dried at 100°C for 24 hours and then calcined at 300°C for 8 hours to obtain a catalyst precursor. 8.9g of boric acid was dissolved in water and impregnated on the above catalyst precursor, dried at 100°C for 15 hours and then calcined at 350°C for 5 hours to obtain a catalyst B, wherein the transition metal oxide and non-metal oxide of the catalyst B were 2% titanium dioxide and 5% boron trioxide, respectively.
[0071] 10 g of catalyst B was loaded into a fixed bed reactor, and the catalyst temperature was raised to 500°C. Ammonia was introduced into the reactor. Propyl acetate was introduced into the reactor at a mass space velocity of 0.1 h -1 The molar ratio of ammonia to propyl acetate was 1:1, and the reaction pressure was 0.5 MPa. The products after the reaction were collected and analyzed, and the conversion rate of propyl acetate was 98.4%, and the selectivity of acetonitrile in the amination product was 99.1wt%.
[0072] Example 3
[0073] 0.3g of ferric nitrate was dissolved in water and impregnated on 84.9g of a formed alumina carrier. After impregnation, it was dried at 120°C for 16 hours and then calcined at 500°C for 4 hours to obtain a catalyst precursor. 20.7g of phosphoric acid was dissolved in water and impregnated on the above catalyst precursor, dried at 120°C for 16 hours and then calcined at 500°C for 4 hours to obtain a catalyst C, wherein the transition metal oxide and non-metal oxide of the catalyst C were 0.1% of ferric oxide and 15% of phosphorus pentoxide, respectively.
[0074] 10 g of catalyst C was loaded into a fixed bed reactor, and the catalyst temperature was raised to 350°C. Ammonia was introduced into the reactor. Methyl acetate was introduced into the reactor at a mass space velocity of 1.5 h -1 The molar ratio of ammonia to methyl acetate was 15:1, and the reaction pressure was 0.1 MPa. The products after the reaction were collected and analyzed, and the conversion rate of methyl acetate was 99.1%, and the selectivity of acetonitrile in the amination products was 99.5wt%.
[0075] Example 4
[0076] 11.8g of copper nitrate was dissolved in water and impregnated on 94.0g of a formed kaolin carrier. After impregnation, it was dried at 120°C for 12 hours and then calcined at 450°C for 6 hours to obtain a catalyst precursor. 1g of selenium dioxide was dissolved in water and impregnated on the above catalyst precursor, dried at 120°C for 12 hours and then calcined at 450°C for 6 hours to obtain a catalyst D, wherein the transition metal oxide and non-metal oxide of the catalyst D were 5% copper oxide and 1% selenium dioxide, respectively.
[0077] 10 g of catalyst D was loaded into a fixed bed reactor, and the catalyst temperature was raised to 400°C. Ammonia was introduced into the reactor. Methyl acetate was introduced into the reactor, and the mass space velocity of methyl acetate was 8.0 h -1 The molar ratio of ammonia to methyl acetate was 40:1, and the reaction pressure was 0.5 MPa. The products after the reaction were collected and analyzed, and the conversion rate of methyl acetate was 97.9%, and the selectivity of acetonitrile in the amination products was 98.2wt%.
[0078] Example 5
[0079] 0.7 g of ammonium heptamolybdate was dissolved in water and impregnated on 88.0 g of a formed alumina carrier. After impregnation, the catalyst was dried at 120° C. for 15 hours and then calcined at 550° C. for 5 hours to obtain a catalyst precursor. 13.8 g of phosphoric acid was dissolved in water and impregnated on the catalyst precursor, dried at 120° C. for 15 hours and then calcined at 550° C. for 5 hours to obtain a catalyst E, wherein the transition metal oxide and non-metal oxide of the catalyst E were 2% molybdenum trioxide and 10% phosphorus pentoxide, respectively.
[0080] 10 g of catalyst E was loaded into a fixed bed reactor, and the catalyst temperature was raised to 350°C. Ammonia was introduced into the reactor. Methyl acetate was introduced into the reactor at a mass space velocity of 3.0 h -1 The molar ratio of ammonia to methyl acetate was 10:1, and the reaction pressure was 0.1 MPa. The products after the reaction were collected and analyzed, and the conversion rate of methyl acetate was 98.6%, and the selectivity of acetonitrile in the amination products was 98.8wt%.
[0081] Example 6
[0082] 4.3g of ammonium dodecotungstate was dissolved in water and impregnated on 81.0g of a formed alumina carrier. After impregnation, it was dried at 120°C for 12 hours, and then calcined at 400°C for 5 hours to obtain a catalyst precursor. 20.7g of phosphoric acid was dissolved in water and impregnated on the above catalyst precursor, dried at 120°C for 12 hours, and then calcined at 400°C for 5 hours to obtain a catalyst F, wherein the transition metal oxide and non-metal oxide of the catalyst F were 4% tungsten trioxide and 15% phosphorus pentoxide, respectively.
[0083] 10 g of catalyst F was loaded into a fixed bed reactor, and the catalyst temperature was raised to 380°C. Ammonia was introduced into the reactor. Methyl acetate was introduced into the reactor at a mass space velocity of 2.0 h -1 The molar ratio of ammonia to methyl acetate was 5:1, and the reaction pressure was 0.2 MPa. The products after the reaction were collected and analyzed, and the conversion rate of methyl acetate was 98.7%, and the selectivity of acetonitrile in the amination products was 99.2wt%.
[0084] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A catalyst for producing acetonitrile, characterized in that The catalyst comprises a transition metal oxide, a non-metal oxide, and a carrier; The content of the transition metal oxide in the catalyst is 0.1-5wt%; The content of the non-metallic oxide in the catalyst is 0.5-30 wt %.
2. The catalyst according to claim 1, characterized in that The content of the transition metal oxide in the catalyst is 1-4wt%; Preferably, the content of the non-metallic oxide in the catalyst is 5-15 wt %.
3. The catalyst according to claim 1, characterized in that The transition metal oxide is selected from at least one of Ti, Mn, Fe, Cu, Mo and W oxides.
4. The catalyst according to claim 1, characterized in that The non-metallic oxide is selected from at least one of oxides of B, P and Se.
5. The catalyst according to claim 1, characterized in that The carrier is selected from at least one of alumina, silica, zirconia and kaolin.
6. The method for preparing the catalyst according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, impregnating an aqueous solution containing a soluble metal salt on a carrier, drying I and then calcining I to obtain a catalyst precursor; S2. Impregnating the catalyst precursor with an aqueous solution containing a soluble non-metallic compound, drying II and then calcining II to obtain the catalyst.
7. The preparation method according to claim 6, characterized in that: The soluble metal salt is selected from at least one of TiCl4, manganese nitrate, manganese acetate, ferric nitrate, ferric sulfate, ferric chloride, copper nitrate, ammonium molybdate, and ammonium tungstate; Preferably, the soluble non-metallic compound is selected from at least one of boric acid, phosphoric acid and selenium dioxide.
8. The preparation method according to claim 6, characterized in that: In step S1, the conditions for drying I are as follows: The temperature is 100-120℃; Time is 12-24h; Preferably, in step S1, the conditions for roasting I are as follows: Temperature is 300-600℃; Time is 3-8h; Preferably, in step S2, the conditions for drying II are as follows: The temperature is 100-120℃; Time is 12-24h; Preferably, in step S2, the conditions for roasting II are as follows: Temperature is 300-600℃; The time is 3-8h.
9. The catalyst according to any one of claims 1 to 5 and / or the catalyst obtained by the preparation method according to any one of claims 6 to 8 is used for the reaction of acetate and ammonia to generate acetonitrile.
10. The use according to claim 9, characterized in that: The molar ratio of the ammonia gas to the acetate is 1-40:1; Preferably, the mass space velocity of the acetate is 0.1-8.0h -1 ; Preferably, the reaction conditions are as follows: Temperature is 250-500℃; Preferably, the reaction pressure is 0.1-0.5 MPa; Preferably, the reaction is carried out in a reactor, and the reactor is selected from at least one of a fixed bed reactor, a tank reactor, a moving bed, and a fluidized bed.