Preparation method and photocatalytic application of MnO / Mn7C3 heterostructure / nitrogen-doped carbon

By preparing MnO/Mn7C3 heterostructure/nitrogen doped carbon, the problem of low efficiency of existing photocatalytic materials when treating dye wastewater is solved, and efficient photocatalytic degradation effect is achieved, especially when treating methylene blue. Degradation efficiency.

CN119016086APending Publication Date: 2024-11-26QINGDAO UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411225147.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing photocatalytic materials are less efficient when treating chemical and printing and dyeing wastewater, especially manganese oxide materials, and are not highly degraded for dye wastewater.

Method used

Using the preparation method of MnO/Mn7C3 heterostructure/nitrogen doped carbon, manganese monoxide, tris(hydroxymethyl)aminomethane and dopamine hydrochloride were stirred in ethanol and water and mixed with melamine, and placed in Ar atmosphere at 450°C. Heating for 1 hour, MnO/Mn7C3 heterostructure/nitrogen doped carbon was prepared and used for photocatalytic degradation of wastewater.

Benefits of technology

The 100% photodegradation efficiency of 1ppm methylene blue was achieved, and the efficiency of photocatalytic degradation of wastewater was significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005024260590000011
    Figure HDA0005024260590000011
Patent Text Reader

Abstract

The invention relates to a preparation method and photocatalytic application of MnO / Mn7C3 heterostructure / nitrogen-doped carbon, and particularly relates to a preparation method of MnO / Mn7C3 heterostructure / nitrogen-doped carbon, which comprises the following steps: dispersing manganese monoxide, tris (hydroxymethyl) aminomethane and dopamine hydrochloride into ethanol and water, stirring, drying, mixing the obtained solid with melamine, and heating in an Ar atmosphere to obtain MnO / Mn7C3 heterostructure / nitrogen-doped carbon; the MnO / Mn7C3 heterostructure / nitrogen-doped carbon prepared by the preparation method is applied to photocatalytic degradation of methylene blue in sewage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and photocatalytic application of a MnO / Mn7C3 heterostructure / nitrogen-doped carbon, and belongs to the field of material preparation and application. Background Art

[0002] With the rapid development of science and technology, people's quality of life has been greatly improved. A large number of chemical, printing and dyeing and other related projects have been built, and the chemical wastewater and domestic wastewater generated are discharged into rivers, which seriously affects people's daily life. In the field of environment, the control of water pollution has become an urgent problem that people need to solve. The commonly used methods at present are: ion exchange method, sedimentation method, adsorption method, photocatalytic degradation method, etc. Among them, photocatalytic degradation technology is to simulate the migration of electrons on semiconductor materials under sunlight, and photogenerated electrons oxidize pollutants to eliminate pollutants.

[0003] At present, the commonly used photocatalytic materials are titanium oxide, tungsten oxide, etc., while there are few reports on manganese oxide. Pung's research group used KMnO4, MnSO4, etc. to synthesize MnO2 nanotubes by hydrothermal treatment at 150℃ for 4h; then used CH3(CH2) 10 CH2SH, MnO2, and PET were used to construct MnO2 nanotubes grown on PET film. When the concentration of Rhodamine B was 1*10 -5mol / L, using MnO2 nanotubes grown on PET film as a catalyst, the photocatalytic efficiency was 90.3% after 120 minutes of visible light catalysis (Journal of Experimental Nanoscience, 2016, 11, 603-618). Doong's research group used melamine, urea, boric acid and L-cysteine ​​to calcine at 550 ° C for 4 hours to obtain B and S co-doped g-C3N4 (CNBS), and then used B and S co-doped g-C3N4, Na2SO4, KMnO4 to synthesize CNBS@MnO2 composites; using CNBS@MnO2 composites as catalysts, photocatalytic degradation of sodium dichloroaniline phenylacetate, the photocatalytic efficiency was 100% after 10 hours of photodegradation (Chemical Engineering Journal, 2023, 452, 139249). Zhou's research group dispersed KMnO4 and MgO in water, stirred at 80°C for 12 hours, then added MnCl2·4H2O solution, stirred for 12 hours, centrifuged, washed, and dried to obtain Mg(OH)2-MnO2 nanocomposite; using Mg(OH)2-MnO2 nanocomposite as catalyst, the photocatalytic efficiency of Congo red solution was 100% after 25 hours of photocatalysis (Separation and Purification Technology, 2021, 272, 118901). Manganese-based oxides have made some progress in the field of photocatalysis. We changed the composition of manganese-based oxides and applied them to photocatalytic reactions to try to photocatalytically degrade dye wastewater. Summary of the invention

[0004] The present invention aims to provide a method for preparing a MnO / Mn7C3 heterostructure / nitrogen-doped carbon.

[0005] Based on the above purpose, the technical solutions involved in the present invention are as follows:

[0006] (1) Preparation of MnO / Mn7C3 heterostructure / nitrogen-doped carbon: 20 mg of manganese monoxide (MnO), 120 mg of tris(hydroxymethyl)aminomethane, and 40-50 mg of dopamine hydrochloride were dispersed in 40 mL of ethanol and 40 mL of water, stirred, and dried. The obtained solid was mixed with 150-200 mg of melamine, and heated at 450°C in an Ar atmosphere for 1 h to obtain MnO / Mn7C3 heterostructure / nitrogen-doped carbon. In the above preparation method, the Mn7C3 is classified as standard card JCPDS#01-089-6159; the MnO is classified as standard card JCPDS#07-0230.

[0007] (2) An application of the MnO / Mn7C3 heterostructure / nitrogen-doped carbon prepared by the above preparation method in photocatalysis, in which 1 ppm of methylene blue in sewage is photocatalytically degraded under illumination for 6-8 hours with a photodegradation efficiency of 100%.

[0008] The present invention has the following advantages:

[0009] (1) A new synthetic route for MnO / Mn7C3 heterostructure / nitrogen-doped carbon is provided.

[0010] (2) MnO / Mn7C3 heterostructure / nitrogen-doped carbon exhibits high catalytic efficiency in photocatalytic degradation of wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 XRD characterization results of MnO / Mn7C3 heterostructure / nitrogen-doped carbon. DETAILED DESCRIPTION

[0012] The following examples are used to further illustrate the present invention, but are not intended to limit the present invention.

[0013] Example 1

[0014] Disperse 20 mg of manganese monoxide (MnO), 120 mg of tris(hydroxymethyl)aminomethane, and 40 mg of dopamine hydrochloride into 40 mL of ethanol and 40 mL of water, stir, and dry. Mix the obtained solid with 150 mg of melamine, and heat it at 450°C in an Ar atmosphere for 1 hour to obtain MnO / Mn7C3 heterostructure / nitrogen-doped carbon. In the above preparation method, the Mn7C3 belongs to the standard card JCPDS#01-089-6159; the MnO belongs to the standard card JCPDS#07-0230. The application of MnO / Mn7C3 heterostructure / nitrogen-doped carbon prepared by the above preparation method in photocatalysis is 100% in the photocatalytic degradation of 1 ppm methylene blue in sewage under illumination for 6 hours.

[0015] Example 2

[0016] Disperse 20 mg of manganese monoxide (MnO), 120 mg of tris(hydroxymethyl)aminomethane, and 50 mg of dopamine hydrochloride in 40 mL of ethanol and 40 mL of water, stir, and dry. Mix the obtained solid with 200 mg of melamine, and heat it at 450°C in an Ar atmosphere for 1 hour to obtain MnO / Mn7C3 heterostructure / nitrogen-doped carbon. In the above preparation method, the Mn7C3 belongs to the standard card JCPDS#01-089-6159; the MnO belongs to the standard card JCPDS#07-0230. An application of MnO / Mn7C3 heterostructure / nitrogen-doped carbon prepared by the above preparation method in photocatalysis, in the photocatalytic degradation of 1 ppm of methylene blue in sewage, the photodegradation efficiency is 100% after 8 hours of illumination.

[0017] Example 3

[0018] 20 mg of manganese monoxide (MnO), 120 mg of tris(hydroxymethyl)aminomethane, and 45 mg of dopamine hydrochloride are dispersed in 40 mL of ethanol and 40 mL of water, stirred, and dried. The obtained solid is mixed with 150 mg of melamine, and heated at 450°C in an Ar atmosphere for 1 h to obtain MnO / Mn7C3 heterostructure / nitrogen-doped carbon. In the above preparation method, the Mn7C3 belongs to the standard card JCPDS#01-089-6159; the MnO belongs to the standard card JCPDS#07-0230. An application of MnO / Mn7C3 heterostructure / nitrogen-doped carbon prepared by the above preparation method in photocatalysis, in the photocatalytic degradation of 1 ppm of methylene blue in sewage, the photodegradation efficiency is 100% after 8 hours of illumination.

Claims

1. A MnO / Mn 7 C 3 Preparation method of heterostructure / nitrogen-doped carbon It is characterized in that The following steps are involved: 20 mg of manganese monoxide (MnO), 120 mg of tris(hydroxymethyl)aminomethane, and 40-50 mg of dopamine hydrochloride were dispersed in 40 mL of ethanol and 40 mL of water, stirred, and dried. The obtained solid was mixed with 150-200 mg of melamine and heated at 450 ° C for 1 h in an Ar atmosphere to obtain MnO / Mn 7 C 3 Heterostructure / nitrogen-doped carbon.

2. The preparation method according to claim 1, It is characterized in that The Mn 7 C 3 It belongs to the standard card JCPDS#01-089-6159, and the MnO belongs to the standard card JCPDS#07-0230.

3. A MnO / Mn prepared by the preparation method according to any one of claims 1 to 2 7 C 3 The application of heterostructure / nitrogen-doped carbon in photocatalysis can achieve 100% photodegradation efficiency for 1 ppm methylene blue in wastewater under 6-8 h of illumination.