Glass-loaded TiO2-BiOCl nano array catalytic material as well as preparation method and application thereof
By growing TiO2-BiOCl nanoarray catalysts on the glass surface, the problems of low cyclohexanol oxidation conversion and difficult catalyst separation are solved, efficient photocatalytic reactions and simplified catalyst recovery process are achieved, and the activity of the catalyst and industrial applications are improved. efficiency.
Patent Information
- Application Number
- CN202411193676.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
Smart Images

Figure CN119056472A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalysts, and particularly relates to a glass-loaded TiO 2 -BiOCl nanoarray catalytic material and its preparation method and application. Background Art
[0002] Cyclohexanol and cyclohexanone are called KA oil in industry. They are key raw materials for producing caprolactam, nylon 6, adipic acid and nylon 66. In industry, cyclohexane oxidation is the mainstream process for producing cyclohexanol and cyclohexanone. However, its conversion rate is only 4%, and the process conditions are thermal catalysis, which needs to be carried out at high temperature and high pressure, and consumes a lot of energy. Therefore, cyclohexane oxidation of KA oil requires the selection of a suitable catalytic process, and needs to develop in the direction of higher activity and atomic economy, mild operating conditions and green oxidants, which can not only meet industrial needs, but also comply with the sustainable development strategy. As an emerging frontier technology, photocatalysis uses green electricity, and has high conversion rate and selectivity.
[0003] To address the problem of low conversion rate, photocatalysts can be modified by ion doping, surface photosensitization, noble metal deposition, semiconductor composites, etc. Among all these methods, the construction of effective heterojunctions is considered to be one of the most feasible strategies to accelerate the transport of photogenerated carriers and effectively inhibit the recombination of photoactivated electron-hole pairs. Traditional powder catalysts have poor dispersibility and thermal stability, are easy to agglomerate, and have fewer reactive active sites.
[0004] CN202410253387.5 discloses a titanium dioxide / bismuth oxychloride heterojunction composite material and a preparation method thereof, S01. A bismuth salt is added to deionized water to obtain a bismuth-containing mixed solution, a sodium hydroxide solution is added, and the pH value of the bismuth-containing mixed solution is adjusted to 3-6 to form a titanium dioxide / bismuth oxychloride heterojunction composite material. 6 O 6 (OH) 3-x ](NO 3 ) 3+x S02, add titanium dioxide nanosphere substrate to suspension A, stir well, and form a suspension containing TiO 2 / [Bi 6 O 6 (OH) 3-x ](NO 3 ) 3+xMixed suspension B of composite precursor; S03, adding sodium chloride and sodium hydroxide to suspension B, adjusting the pH value of the suspension to 9-13, and obtaining mixed suspension C; S04. Hydrothermal reaction, reacting mixed suspension C at a specified temperature for a specified time and then cooling naturally to obtain a semi-finished titanium dioxide / bismuth oxychloride heterojunction composite material; S05. Washing the semi-finished titanium dioxide / bismuth oxychloride heterojunction composite material to neutrality and drying to obtain a finished titanium dioxide / bismuth oxychloride heterojunction composite material; However, the material synthesized using deionized water cannot control the morphology and crystal plane and cannot introduce oxygen vacancies, and the morphology of bismuth oxychloride is closely related to the separation and transfer of photogenerated carriers and photocatalytic performance. Bismuth oxychloride rich in oxygen vacancies can significantly expand the visible light response to the visible / infrared band, and induce the generation of local polarization to attract photogenerated holes, thereby improving the separation efficiency of photogenerated carriers. Bulk bismuth oxychloride catalysts suffer from poor photon absorption, long carrier diffusion lengths, and poor crystal quality, resulting in suboptimal photocatalytic activity. Summary of the invention
[0005] In view of the problems existing in the prior art, the first purpose of the present invention is to provide a composite photothermal nanoarray catalytic material, which increases the photocatalytic activity, promotes rapid charge migration, reduces the recombination rate of photogenerated holes and electrons, and at the same time increases the contact area between the catalyst and the reactants, improves the catalytic activity, and addresses the problem of low reaction conversion rate; at the same time, the form of glass-loaded nanoarrays also solves the problem of difficulty in separating the reaction products and powdered catalysts.
[0006] The second object of the present invention is to provide a glass-loaded TiO 2 -Preparation method of BiOCl nanoarray catalytic material.
[0007] The third object of the present invention is to provide a glass-loaded TiO prepared by the above preparation method. 2 -BiOCl nanoarray catalytic material.
[0008] The fourth object of the present invention is to provide the glass-loaded TiO 2 -Application of BiOCl nanoarray catalytic materials in catalytic cyclohexane oxidation.
[0009] To this end, the first technical solution provided by the present invention is as follows:
[0010] A glass loaded TiO 2 -The preparation method of BiOCl nano-array catalytic material comprises the following steps in sequence:
[0011] S1. Preparation of TiO 2 Nanoarray
[0012] Add titanium source to deionized water and adjust the pH of the solution to acidic to obtain precursor solution A. Place the conductive glass obliquely into the prepared precursor solution A and perform hydrothermal reaction at 160-200°C for 1-10h. The reaction product is ultrasonicated, cleaned, and naturally air-dried to obtain TiO 2 Conductive glass with nanoarrays;
[0013] S2. Preparation of TiO 2 -BiOCl composites
[0014] Bismuth source and chlorine source are added to ethylene glycol, and then mannitol is added to obtain precursor solution B. The TiO 2 The conductive glass of the nanoarray is placed in a polytetrafluoroethylene liner, and then the precursor solution B is added. The reaction is carried out at 150-170°C for 1-12 hours. The reaction product is ultrasonically cleaned, naturally air-dried, and then irradiated under a 365nm ultraviolet lamp for 10-60 minutes to obtain glass-loaded TiO 2 -BiOCl composite nanomaterials;
[0015] The molar ratio of the titanium source, the bismuth source and the chlorine source is: 2-4:1.5-2.5:2-4.
[0016] Furthermore, the above-mentioned glass-loaded TiO 2 -Method for preparing BiOCl nanoarray catalytic material, wherein the titanium source in step S1 is tetrabutyl titanate.
[0017] Furthermore, the above-mentioned glass-loaded TiO 2 -A method for preparing a BiOCl nanoarray catalytic material, wherein in step S1, hydrochloric acid is used to adjust the pH value of the solution to acidity; the concentration of the hydrochloric acid solution is 5 mol / L; and the pH value is 5.
[0018] Furthermore, the above-mentioned glass-loaded TiO 2 -Method for preparing BiOCl nano-array catalytic material, the molar ratio of the titanium source and hydrochloric acid in step S1 is 1:4 to 1:50.
[0019] Furthermore, the above-mentioned glass-loaded TiO 2 - A method for preparing a BiOCl nanoarray catalytic material, wherein the bismuth source in step S2 is a bismuth nitrate pentahydrate solution with a concentration of 40 mmol / L to 120 mmol / L; and the chlorine source is a 0.2 mol / L potassium chloride solution.
[0020] Furthermore, the above-mentioned glass-loaded TiO 2 -The preparation method of BiOCl nanoarray catalytic material, the cleaning described in steps S1 and S2 uses acetone as the cleaning agent.
[0021] The second technical solution provided by the present invention is a glass loaded TiO 2 -BiOCl nanoarray catalytic material, prepared by the method described in the first technical solution.
[0022] The third technical solution provided by the present invention is the glass-loaded TiO 2 -BiOCl nanoarray catalytic material is used for photothermal catalytic cyclohexane oxidation reaction.
[0023] The fourth technical solution provided by the present invention is a glass-loaded TiO 2 -BiOCl nano-array catalytic material catalyzes the photothermal catalytic cyclohexane oxidation reaction, wherein the glass-loaded TiO 2 -BiOCl nanoarray catalytic material is dissolved in a mixture of cyclohexane and acetonitrile, with the catalyst side facing upward; the reaction time is 6-10 hours under dry air pressure of 1.0-2.0MPa and 100-150°C; the reaction light source is the ultraviolet partial area light source of a xenon lamp.
[0024] Furthermore, the above-mentioned glass-loaded TiO 2 -A method for photothermal catalytic cyclohexane oxidation reaction using BiOCl nano-array catalytic materials, wherein the wavelength of the light source is 300-780nm.
[0025] Compared with the prior art, the technical solution provided by the present invention has the following technical advantages:
[0026] 1. A glass-loaded TiO prepared by the present invention 2 -BiOCl nanoarray catalytic material, by 2 BiOCl nanosheets are grown on the nanorod array to form a heterostructure, allowing its electrons to be transferred from the photocatalyst TiO 2 Transferred to BiOCl, the nesting of nanoarray composite nanorods and nanosheets can maximize the contact area between the catalyst and the reactants. The in-situ increased oxygen vacancy content after UV light treatment improves the photocatalytic activity and solves the problem of low reaction conversion rate. At the same time, growing the catalyst on the glass surface can avoid the problem of subsequent separation of the catalyst and save process costs.
[0027] 2. The technical solution provided by the present invention significantly improves the light absorption efficiency by optimizing the nanoarray structure, thereby improving the catalytic efficiency of the photocatalytic reaction. In addition, a double-layer nested design is adopted, combining different nanomorphologies (such as nanoarray nanorods and nanosheets) to achieve efficient catalyst compounding. At the same time, after a simple ultraviolet light treatment, BiOCl generates oxygen vacancies in situ, effectively improving the photocatalytic activity.
[0028] 3. The technical solution provided by the present invention grows the catalyst directly on the glass surface. This design not only simplifies the catalyst fixation and recovery process, but also provides a convenient and efficient idea for the subsequent separation of cyclohexane oxidation products. The catalyst and the product can be effectively separated by simple physical separation means, which greatly reduces the complexity and cost of subsequent treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 TiO loaded on glass 2 -Schematic diagram of the structure of BiOCl nanoarray catalytic material;
[0030] Figure 2 This is the SEM morphology of the TiO2 nanorod array catalytic material;
[0031] Figure 3 This is the XRD pattern of TiO2 nanorod array catalytic material;
[0032] Figure 4 TiO 2 -SEM morphology of BiOCl nanocomposite array catalytic materials;
[0033] Figure 5 TiO 2 - EDS and mapping of components of BiOCl nanocomposite array catalytic materials;
[0034] Figure 6 TiO 2 -Element content analysis diagram of BiOCl nanocomposite array catalytic material;
[0035] Figure 7 TiO 2 、BiOCl、TiO 2 -Structural characterization XRD diagram of BiOCl nanocomposite array catalytic material;
[0036] Figure 8 TiO 2 、BiOCl、TiO 2 - Raman images of BiOCl nanocomposite array catalytic materials;
[0037] Fig. 9 TiO 2 、BiOCl、TiO 2 -BiOCl, TiO 2 -UV-vis graph of BiOCl-light nanocomposite array catalytic material performance test;
[0038] Fig.10 TiO2 , Performance test band gap diagram of BiOCl catalytic material;
[0039] Fig.11 TiO 2 Mott-Schottky plot of performance test of catalytic materials;
[0040] Fig.12 Mott-Schottky plot for the performance test of BiOCl catalytic materials;
[0041] Fig.13 TiO 2 - Performance comparison of BiOCl-light nanocomposite array catalytic materials in photocatalytic, thermal and photothermal catalytic cyclohexane oxidation reactions
[0042] Fig.14 TiO 2 、TiO 2 -BiOCl-light, TiO 2 - Performance comparison of BiOCl nanocomposite array catalytic materials used in photothermal catalytic cyclohexane oxidation reaction
[0043] Fig.15 TiO 2 - Gas chromatogram of BiOC-light composite nanoarray catalyst applied to photothermal catalytic cyclohexane oxidation reaction;
[0044] Fig.16 TiO 2 -Gas chromatogram of BiOC-light composite nanoarray catalyst applied to thermal catalytic cyclohexane oxidation reaction.
[0045] Fig.17 TiO 2 - Gas chromatogram of BiOC-light composite nanoarray catalyst applied to photocatalytic cyclohexane oxidation reaction;
[0046] Fig.18 TiO 2 Gas chromatogram of photocatalyst applied to thermal cyclohexane oxidation reaction;
[0047] Fig.19 TiO 2 Gas chromatogram of photocatalyst applied to photothermal catalytic cyclohexane oxidation reaction;
[0048] Fig. 20 TiO 2 -Gas chromatogram of BiOCl powder catalyst applied to photothermal catalytic cyclohexane oxidation reaction. DETAILED DESCRIPTION
[0049] The claims of the present invention are further described in detail below in conjunction with specific embodiments, but do not constitute any limitation to the present invention. Any limited modifications made by anyone within the scope of the claims of the present invention are still within the scope of the claims of the present invention.
[0050] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the present technical field.
[0051] Example 1
[0052] This embodiment provides a glass-loaded TiO 2 -BiOCl nanoarray catalytic material, which is prepared by the following steps in sequence:
[0053] 1) Glass-loaded TiO 2 Nanoarray preparation method
[0054] 20 mL of deionized water and 20 mL of concentrated hydrochloric acid were mixed and stirred, and then 1.3 mL of tetrabutyl titanate was added dropwise and stirred for 30 min to obtain precursor solution A. The prepared FTO conductive surface was immersed in a polytetrafluoroethylene liner containing precursor solution A with the surface facing down, and heated in an oven at 180 ° C for 1 h. After cooling to room temperature, it was ultrasonically washed with deionized water for 10 min and naturally air-dried to obtain the loaded TiO 2 Nanorod arrays on FTO conductive glass.
[0055] 2) Glass-loaded TiO 2 - Preparation method of BiOCl composite catalytic material
[0056] Dissolve 0.48 g of bismuth nitrate pentahydrate and 0.55 g of mannitol in 30 mL of ethylene glycol, then add 5 mL of 0.2 mol / L potassium chloride solution dropwise, and stir in a water bath at 75 °C for 30 min to obtain precursor solution B. 2 The conductive surface of the FTO conductive glass of the nanorod array was immersed in a polytetrafluoroethylene liner containing precursor solution B with the conductive surface facing downward, heated to 160 °C for 3 h, cooled to room temperature, and ultrasonically washed for 10 min with a mixture of deionized water and acetone in a volume ratio of 1:5, naturally air-dried, and then irradiated with 365 nm ultraviolet light for 30 min to obtain the loaded TiO 2 -BiOCl composite catalytic material conductive glass, denoted as TiO 2 -BiOCl-light.
[0057] Sample characterization:
[0058] Step 1) Prepared TiO 2 XRD of nanoarrays ( Figure 2 ) confirmed that it is TiO 2The rutile phase of TiO 2 The band gap width is 2.92eV ( Fig.10 , 11 ); SEM morphology confirmed that it is a tetragonal system ( Figure 1 ).
[0059] Step 2) Prepared TiO 2 -The EDS and mapping images of BiOCl nanocomposite array catalytic materials show that Bi and Cl elements are evenly distributed on the TiO 2 Nanoarray Figure 3 , Figure 4 ), the morphology SEM confirmed that BiOCl was loaded on TiO in the form of nanosheets. 2 Nanoarray top ( Figure 3 ). XRD patterns confirmed that TiO 2 -BiOCl nanocomposite array catalytic materials have been successfully prepared, see Figure 7 , UV spectrum and Mott Schottky potential diagram show that the band gap width of BiOCl is 3.38eV ( Fig.10 , 12 ), and confirmed that TiO 2 -BiOCl forms a type II heterojunction.
[0060] Example 2
[0061] This embodiment provides a glass-loaded TiO 2- The preparation method of BiOCl nano-array catalytic material comprises the following steps:
[0062] 1) TiO 2 Nanoarray preparation method
[0063] 20 mL of deionized water and 20 mL of concentrated hydrochloric acid were mixed and stirred, and then 1.3 mL of tetrabutyl titanate was added dropwise and stirred for 30 min to obtain precursor solution A. The prepared FTO conductive surface was immersed in a polytetrafluoroethylene liner containing precursor solution A with the surface facing down, heated in an oven at 180 ° C for 1 h, cooled to room temperature, ultrasonically washed with deionized water for 10 min, and naturally air-dried to obtain a loaded TiO 2 Nanorod arrays on FTO conductive glass.
[0064] 2) TiO 2 - Preparation method of BiOCl composite catalytic material
[0065] Dissolve 0.48 g of bismuth nitrate pentahydrate and 0.55 g of mannitol in 30 mL of ethylene glycol, then add 5 mL of 0.2 mol / L potassium chloride solution dropwise, and stir in a water bath at 75 °C for 30 min to obtain precursor solution B. 2 The conductive surface of the FTO conductive glass of the nanorod array was immersed in a polytetrafluoroethylene liner containing precursor solution B with the conductive surface facing downward, heated to 160°C for 3 h, cooled to room temperature, ultrasonically washed with a mixture of deionized water and acetone in a volume ratio of 1:5 for 10 min, naturally air-dried, and then irradiated with 365 nm ultraviolet light for 30 min to obtain the loaded TiO 2 -BiOCl composite catalytic material conductive glass, denoted as TiO 2 -BiOCl-light.
[0066] Example 3
[0067] This embodiment provides a glass-loaded TiO 2 -The preparation method of BiOCl nano-array catalytic material comprises the following steps:
[0068] 1) TiO 2 Nanoarray preparation method
[0069] 20 mL of deionized water and 20 mL of concentrated hydrochloric acid were mixed and stirred, and then 1.3 mL of tetrabutyl titanate was added dropwise and stirred for 30 min to obtain precursor solution A. The prepared FTO conductive surface was immersed in a polytetrafluoroethylene liner containing precursor solution A with the surface facing down, heated in an oven at 180 ° C for 1 h, cooled to room temperature, ultrasonically washed with deionized water for 10 min, and naturally air-dried to obtain a loaded TiO 2 Nanorod arrays on FTO conductive glass.
[0070] 2) TiO 2 - Preparation method of BiOCl composite catalytic material
[0071] Dissolve 0.96 g of bismuth nitrate pentahydrate and 0.55 g of mannitol in 30 mL of ethylene glycol, then add 5 mL of 0.2 mol / L potassium chloride solution dropwise, and stir in a water bath at 75 °C for 30 min to obtain precursor solution B. 2 The conductive surface of the FTO conductive glass of the nanorod array was immersed in a polytetrafluoroethylene liner containing precursor solution B with the conductive surface facing downward, heated to 160°C for 3 h, cooled to room temperature, and then ultrasonically washed with a mixture of deionized water and acetone in a volume ratio of 1:5 for 10 min, naturally air-dried, and then irradiated with 365 nm ultraviolet light for 30 min to obtain the loaded TiO 2 -BiOCl composite catalytic material conductive glass, denoted as TiO 2 -BiOCl-light.
[0072] Example 4
[0073] This embodiment provides a glass-loaded TiO 2 -The preparation method of BiOCl nano-array catalytic material comprises the following steps:
[0074] 1) TiO 2 Nanoarray preparation method
[0075] 20 mL of deionized water and 20 mL of concentrated hydrochloric acid were mixed and stirred, and then 1.3 mL of tetrabutyl titanate was added dropwise and stirred for 30 min to obtain precursor solution A. The prepared FTO conductive surface was immersed in a polytetrafluoroethylene liner containing precursor solution A with the surface facing down, heated in an oven at 180 ° C for 1 h, cooled to room temperature, ultrasonically washed with deionized water for 10 min, and naturally air-dried to obtain a loaded TiO 2 Nanorod arrays on FTO conductive glass.
[0076] 2) TiO 2 - Preparation method of BiOCl composite catalytic material
[0077] 0.24 g of bismuth nitrate pentahydrate and 0.55 g of mannitol were dissolved in 30 mL of ethylene glycol, and then 5 mL of 0.2 mol / L potassium chloride solution was added dropwise, and stirred in a water bath at 75°C for 30 min to obtain precursor solution B. The FTO conductive glass loaded with TiO2 nanorod array prepared in step 1) was immersed in a polytetrafluoroethylene liner filled with precursor solution B with the conductive surface facing downward, heated to 160°C for reaction for 3 h, cooled to room temperature, and ultrasonically washed with a mixture of deionized water and acetone in a volume ratio of 1:5 for 10 min, naturally air-dried, and then irradiated with 365 nm ultraviolet light for 30 min to obtain a TiO2 nanorod array loaded with FTO conductive glass. 2 -BiOCl composite catalytic material conductive glass, denoted as TiO 2 -BiOCl-light.
[0078] Application Example 1
[0079] This application example uses the glass-loaded TiO provided in Example 1. 2 -BiOCl-light composite nanoarray catalytic material catalyzes the photothermal catalytic reaction of cyclohexane, and the reaction process specifically includes the following steps:
[0080] 8 mg of TiO 2 -The conductive glass of BiOCl-light composite photothermal catalytic material was dissolved in a mixture of 7mL of cyclohexane and 8mL of acetonitrile, with the catalyst side facing upwards;
[0081] Reaction conditions: reaction pressure is 1.5MPa dry air pressure, reaction temperature is 120°C; reaction time is 8h; reaction light source is ultraviolet partial area light source (300-780nm) of xenon lamp;
[0082] After the reaction was completed, the product was detected by gas chromatography, and the contents of cyclohexanol and cyclohexanone were determined by the internal standard method. The conversion rate was calculated to be 10.62% and the selectivity was 98.60%.
[0083] Application Example 2
[0084] This application example uses the glass-loaded TiO provided in Example 2 2 -BiOCl nanoarray catalytic material catalyzes the photothermal catalytic reaction of cyclohexane, and the reaction process specifically includes the following steps:
[0085] 8 mg of TiO 2 -The conductive glass of BiOCl composite photothermal catalytic material was dissolved in a mixture of 7mL of cyclohexane and 8mL of acetonitrile, with the catalyst side facing upwards;
[0086] Reaction conditions: reaction pressure is 1.5MPa dry air pressure, reaction temperature is 120°C; reaction time is 8h; reaction light source is the ultraviolet partial area light source (300-780nm) of xenon lamp;
[0087] After the reaction was completed, the product was detected by gas chromatography, and the contents of cyclohexanol and cyclohexanone were determined by the internal standard method. The calculated conversion rate was 8.92% and the selectivity was 98.52%.
[0088] Comparative application example 1
[0089] This comparative application example adopts the loaded TiO 2 The FTO conductive glass of the nanorod array catalyzes the photothermal catalytic reaction of cyclohexane, and the reaction process specifically includes the following steps:
[0090] 8 mg of TiO 2 The conductive glass of the nanoarray catalytic material was dissolved in a mixture of 7 mL of cyclohexane and 8 mL of acetonitrile, with the side with the catalyst facing upwards;
[0091] Reaction conditions: reaction pressure is 1.5MPa dry air pressure, reaction temperature is 120°C; reaction time is 8h; reaction light source is the ultraviolet partial area light source (300-780nm) of xenon lamp;
[0092] After the reaction was completed, the product was detected by gas chromatography, and the contents of cyclohexanol and cyclohexanone were determined by the internal standard method. The conversion rate was calculated to be 6.98% and the selectivity was 98.11%.
[0093] Comparative Application Example 2
[0094] This application example uses the glass-loaded TiO provided in Example 1. 2 -BiOCl nanoarray catalytic material catalyzes the thermal catalytic reaction of cyclohexane, and the reaction process specifically includes the following steps:
[0095] 8 mg of TiO 2 -The conductive glass of BiOCl composite photothermal catalytic material was dissolved in a mixture of 7mL of cyclohexane and 8mL of acetonitrile, with the catalyst side facing upwards;
[0096] Reaction conditions: reaction pressure is 1.5 MPa dry air pressure, reaction temperature is 120°C; reaction time is 8 h.
[0097] After the reaction, the product was detected by gas chromatography, and the contents of cyclohexanol and cyclohexanone were determined by the internal standard method. The conversion rate was calculated to be 7.81%, and the selectivity was 98.27%. The sample was recorded as TiO 2 -BiOCl-TC.
[0098] Comparative Application Example 3
[0099] This application example uses the glass-loaded TiO provided in Example 1. 2 -BiOCl nano-array catalytic material catalyzes the photocatalytic reaction of cyclohexane, and the reaction process specifically includes the following steps:
[0100] Loading TiO 2 -The conductive glass of BiOCl composite photocatalytic material was dissolved in a mixture of 7 mL of cyclohexane and 8 mL of acetonitrile, with the catalyst side facing upwards;
[0101] Reaction conditions: reaction pressure is 1.5 MPa dry air pressure, reaction temperature is room temperature; reaction time is 8 hours; reaction light source is the ultraviolet partial area light source (300-780 nm) of a xenon lamp.
[0102] After the reaction was completed, the product was detected by gas chromatography, and the contents of cyclohexanol and cyclohexanone were determined by the internal standard method. The calculated conversion rate was 0.35% and the selectivity was 62.17%.
[0103] Comparative Application Example 4
[0104] 0.48 g BiCl 3 Dissolved in TiO 2 The carrier was immersed in pure water at 200W ultrasound for 4 hours, dried at 110℃, and calcined at 450℃ for 2 hours to obtain TiO 2 -BiOCl powder catalyst. The same mass of TiO 2-BiOCl powder catalyst was dissolved in a mixture of 7 mL of cyclohexane and 8 mL of acetonitrile;
[0105] Reaction conditions: reaction pressure is 1.5MPa dry air pressure, reaction temperature is 120℃; reaction time is 8h; reaction light source is ultraviolet partial area light source of xenon lamp (300-780nm)
[0106] After the reaction, the product was tested by gas chromatography, and the contents of cyclohexanol and cyclohexanone were determined by the internal standard method. The conversion rate was calculated to be 7.98% and the selectivity was 98.62%.
[0107] Through the above application examples and comparative application examples, it can be seen that compared with TiO 2 Nanoarray, TiO 2 -BiOCl composite catalyst, TiO in Application Example 1 2 -BiOCl-light composite catalyst has a photothermal cyclohexane oxidation conversion rate of pure TiO 2 1.52 times of that under photothermal conditions and pure thermal conditions, TiO 2 The conversion rate of the -BiOCl composite photothermal catalytic material is 1.36 times different under pure light conditions, and 30.64 times different under pure light conditions, which also confirms that the effect of photothermal synergy is better than any single condition. Compared with the powder catalyst and the nanoarray catalyst, under the same catalyst, the conversion rate of the nanoarray structure is 1.33 times that of the powder structure, indicating that the array structure is better than the powder structure.
Claims
1. A glass loaded TiO 2 - Preparation method of BiOCl nanoarray catalytic material, It is characterized in that The following steps are included in sequence: S1. Preparation of TiO 2 Nanoarray Add titanium source to deionized water and adjust the pH of the solution to acidic to obtain precursor solution A. Place the conductive glass obliquely into the prepared precursor solution A and perform hydrothermal reaction at 160-200°C for 1-10h. The reaction product is ultrasonicated, cleaned, and naturally air-dried to obtain TiO 2 Conductive glass with nanoarrays; S2. Preparation of TiO 2 -BiOCl composites Bismuth source and chlorine source are added to ethylene glycol, and then mannitol is added to obtain precursor solution B. The TiO 2 The conductive glass of the nano-array is placed in a polytetrafluoroethylene liner, and then the precursor solution B is added. The solvent thermal reaction is carried out at 150-170°C for 1-12 hours. The reaction product is ultrasonically cleaned, naturally air-dried, and then irradiated under ultraviolet light for 10-60 minutes to obtain glass-loaded TiO 2 -BiOCl composite nanomaterials; The molar ratio of the titanium source, the bismuth source and the chlorine source is: 2-4:1.5-2.5:2-4.
2. A glass-loaded TiO according to claim 1 2 - Preparation method of BiOCl nanoarray catalytic material, It is characterized in that The titanium source described in step S1 is tetrabutyl titanate.
3. A glass-loaded TiO according to claim 1 2 - Preparation method of BiOCl nanoarray catalytic material, It is characterized in that In step S1, hydrochloric acid is used to adjust the pH value of the solution to acidity; the concentration of the hydrochloric acid solution is 5 mol / L; and the pH value is 5.
4. A glass-loaded TiO according to claim 3 2 - Preparation method of BiOCl nanoarray catalytic material, It is characterized in that The molar ratio of the titanium source and the hydrochloric acid in step S1 is 1:4 to 1:
50.
5. A glass-loaded TiO according to claim 1 2 - Preparation method of BiOCl nanoarray catalytic material, It is characterized in that The bismuth source in step S2 is a bismuth nitrate pentahydrate solution with a concentration of 40 mmol / L to 120 mmol / L; the chlorine source is a 0.2 mol / L potassium chloride solution.
6. A glass-loaded TiO according to claim 1 2 - Preparation method of BiOCl nanoarray catalytic material, It is characterized in that The cleaning in steps S1 and S2 uses acetone as a cleaning agent.
7. A glass loaded TiO 2 -BiOCl nanoarray catalytic materials, It is characterized in that The method is prepared by any one of claims 1 to 6.
8. The glass-loaded TiO according to claim 7 2 -BiOCl nanoarray catalytic material is used for photothermal catalytic cyclohexane oxidation reaction.
9. A glass loaded TiO 2 - A method for photothermal catalytic cyclohexane oxidation reaction catalyzed by BiOCl nano-array catalytic materials, It is characterized in that The glass according to claim 7 is loaded with TiO 2 -BiOCl nanoarray catalytic material is dissolved in a mixture of cyclohexane and acetonitrile, with the catalyst side facing upward; the reaction time is 6-10 hours under dry air pressure of 1.0-2.0MPa and 100-150°C; the reaction light source is the ultraviolet partial area light source of a xenon lamp.
10. A glass-loaded TiO according to claim 9. 2 - A method for photothermal catalytic cyclohexane oxidation reaction catalyzed by BiOCl nano-array catalytic materials, It is characterized in that The wavelength of the light source is 300-780nm.
Citation Information
Patent Citations
Method for synthesizing titanium dioxide / bismuth oxychloride composite electrode on FTO
CN103643254A
Polymeric Coatings Incorporating Bioactive Enzymes for Cleaning a Surface
US20110240064A1
Cited By
BiOCl / TiO2 composite film with amphiphilic surface as well as preparation method and application of BiOCl / TiO2 composite film
CN119771186A
A biocl / tio2 composite film with an amphiphilic surface and a preparation method and application thereof
CN119771186B
Method for producing coatings from bismuth oxychloride layers on oxidized titanium
RU2867317C1