Calcium and siliceous mineral composite inhibitor for separation of blast furnace gravitational fly ash and preparation method of calcium and siliceous mineral composite inhibitor
By using a composite inhibitor of calcium and silicon minerals in the ash separation of blast furnace gravity dust collectors, the problem of reduced calorific value of carbon powder caused by high calcium and silicon content was solved, achieving efficient separation and improving the grade and calorific value of carbon powder and iron concentrate.
Patent Information
- Application Number
- CN202411319992.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-26
AI Technical Summary
After the blast furnace gravity dust is treated, the calcium and silicon content in the product is high, which leads to a decrease in the calorific value of the carbon powder and affects its subsequent utilization.
A composite inhibitor of calcium and silicon minerals is used, which combines inorganic and organic inhibitors to adsorb onto the surface of calcium and silicon minerals, increasing their hydrophilicity, reducing their adhesion to the toner surface, improving sorting efficiency, and obtaining high-grade toner and iron concentrate.
It effectively improves the grade and calorific value of toner, reduces ash content, and increases the economic benefits of enterprises. The grade of iron concentrate is improved, the calorific value of toner increases from 5760 kcal to 6554 kcal, the ash content decreases from 25% to 16.99%, and the volatile matter decreases from 3% to 1.08%.
Smart Images

Figure BDA0005053575940000011 
Figure BDA0005053575940000071 
Figure BDA0005053575940000081
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of blast furnace gravity dust removal ash sorting, and in particular to a silicon-calcium composite inhibitor and a preparation method thereof, in particular to a calcium-silicon mineral composite inhibitor for blast furnace gravity dust removal ash sorting and a preparation method thereof. Background Art
[0002] Blast furnace gravity dust is produced during the smelting process of the blast furnace. The volatile vapor (such as alkali metal salts, zinc, lead, tin, etc.) and sintered ore, pelletized ore and other ores, coke, other gangue, stripped blast furnace lining and other tiny particles are carried out of the blast furnace by the blast furnace gas flow from the top of the blast furnace, and are captured by the coal gas dust removal and purification system composed of gravity dust collectors, bag dust collectors and other dust removal equipment. It consists of 25-45wt% of total iron, 15-40wt% of fixed carbon, 5-10wt% of alkali metal elements and alkaline earth metals such as K2O, Na2O, CaO, MgO, etc., and there are also 0-5wt% Zn and its compounds and other elements in balance. The composition analysis of gravity dust of a steel plant is shown in Table 1 below. The main phases of blast furnace gravity dust removal ash are hematite (Fe2O3), potassium chloride (KCl), zinc oxide (ZnO), calcium feldspar (CaO·Al2O3·2SiO2) and fixed carbon.
[0003] Table 1 Main chemical composition of blast furnace gravity dust removal ash (%)
[0004]
[0005] At present, there are several main ways to utilize the blast furnace gravity dust: First, it is directly returned to sintering for batching, and the iron in the dust ash is used, and then the fixed carbon in it is used as sintering fuel, which effectively reduces the sintering energy consumption. However, if the amount of dust ash added to the sintering material is too large, it will easily cause poor permeability of the material column and reduced strength of the sintered ore. In addition, it will also cause the circulation and enrichment of zinc in the blast furnace, seriously affecting the safe and smooth operation of the blast furnace. The second is pyrometallurgical treatment, using rotary kilns, rotary hearth furnaces, etc. at a certain high temperature, using the carbon in the dust ash as a reducing agent and fuel, to reduce the iron oxides in the dust ash to obtain metallic iron or produce sponge iron, and zinc and other precious metals are enriched through the reduction and oxidation process, collected through the dust removal system, and further processed to prepare zinc ingots. The third is to use the ore dressing enrichment method, that is, using flotation agents to float the carbon powder with a lower density in the dust ash, and the iron with a higher density is selected through magnetic separation and gravity separation.
[0006] CN201910754389 discloses a method for recovering zinc, iron and / or carbon from blast furnace gas ash, wherein the blast furnace gas ash is modulated into a slurry, and a 0.025mm-level wet screening is performed to obtain zinc-containing particles with a particle size less than 0.025mm and iron-containing and carbon-containing materials with a particle size of more than 0.025mm; the obtained iron-containing and carbon-containing materials are spirally sorted, and dehydrated after the sorting is completed to obtain carbon products and iron products. The present invention divides the blast furnace gas ash into zinc-containing particles and iron-containing and carbon-containing materials by 0.025mm-level wet screening, and selects spiral sorting to sort iron and carbon according to the density difference between iron and carbon and the particle size characteristics of the iron-containing and carbon-containing materials, thereby realizing the separation and recovery of zinc, iron and / or carbon in the blast furnace gas ash, the zinc content in the zinc-rich product is as high as 6.01wt%, the iron content in the iron product is as high as 50.45wt%, and the carbon content in the carbon product is as high as 51.14wt%.
[0007] CN201110232076 discloses a process for recovering iron and carbon elements from blast furnace gas ash, adopting flotation method to recover carbon, adopting gravity and magnetic separation method to recover iron, and the overall separation process is "flotation, gravity-magnetic separation combined process flow": gas ash is fed into rough flotation after slurry mixing and reagent addition, rougher concentrate is fed into fine flotation, fine flotation concentrate is the final carbon concentrate, rougher flotation tailings and fine flotation tailings are fed into rougher spiral flow trough of gravity separation, gravity separation tailings are thrown out, rougher spiral concentrate is fed into fine spiral flow trough of gravity separation to obtain gravity separation concentrate, fine spiral middlings are self-circulated, fine spiral tailings are fed into weak magnetic separator for magnetic separation, weak magnetic concentrate and gravity separation concentrate are combined into final iron concentrate, weak magnetic tailings and gravity separation tailings are combined into final tailings. The beneficial effects are: simple process, fewer reagent varieties, reasonable process configuration, significant purification and impurity removal effects, better product quality, high recovery rate, and provide a new way for the comprehensive utilization of blast furnace gas ash.
[0008] CN201910978959 discloses a method for recovering carbon, iron and zinc from blast furnace gas ash. (1) Mixing gas ash with a collector and a frother; (2) Roughing the mixed slurry to obtain carbon concentrate and roughing tailings; (3) Adding a collector and a frother to the roughing tailings for scavenging to obtain carbon concentrate and scavenging tailings; (4) Grinding the scavenging tailings, feeding them into a hydrocyclone for classification, and obtaining sedimentation and overflow products; (5) Feeding the overflow products into a hydrocyclone for classification, and obtaining overflow products and sedimentation; (6) Obtaining zinc concentrate from the overflow products, and magnetically separating the sedimentation to obtain iron concentrate. The method can simultaneously recover the useful components of carbon, iron and zinc in blast furnace gas ash, and the tailings can be used as raw materials for producing cement, thereby realizing the comprehensive utilization of blast furnace gas ash; and the method has the characteristics of low energy consumption, low pollution, high zinc removal rate and low cost.
[0009] The above methods can alleviate the pressure of blast furnace gravity dust removal on the ecological environment, but there are also problems that need to be improved: for example, the calorific value of carbon powder is reduced and the calorific value is reduced.
[0010] In summary, the prior art has at least the following problems: after the blast furnace gravity dust removal ash is processed and recovered, the calcium and silicon content in the product is high and the calorific value of the carbon powder is reduced. Summary of the invention
[0011] The present invention provides a silicon-calcium composite inhibitor and a preparation method thereof, in particular, a calcium-siliceous mineral composite inhibitor for blast furnace gravity dust separation and a preparation method thereof, so as to at least solve the problem that after the blast furnace gravity dust is processed and recovered, the calcium-silicon content in the product is high and the calorific value of carbon powder is reduced.
[0012] To this end, the present invention proposes a calcium and silicon mineral composite inhibitor for blast furnace gravity dust separation, and the mineral composite inhibitor comprises, by weight:
[0013] 10-100 parts of deionized water, 0.1-100 parts of inorganic inhibitors, 0.1-100 parts of organic inhibitors.
[0014] Furthermore, the inorganic inhibitor includes one or more of water glass, sodium carbonate, sodium bicarbonate and phosphates.
[0015] Furthermore, the water glass modulus is 2.2-3.0.
[0016] Furthermore, the organic inhibitor includes one or more of tannin, lignin sulfonate, amino enzymatic lignin, tartaric acid, oxalic acid, carboxymethyl cellulose and starch.
[0017] The present invention also provides a method for preparing a composite inhibitor of calcium and silicon minerals for separation of blast furnace gravity dust removal ash, comprising the following steps:
[0018] Step S1: weighing a certain amount of deionized water;
[0019] Step S2: weigh a certain amount of inorganic inhibitor, add it into the deionized water in step S1, stir it at 1000-2000 r / min for 30-60 min to completely dissolve it, and obtain an inorganic inhibitor solution;
[0020] Step S3: weigh a certain amount of organic inhibitor, and add it into the inorganic inhibitor solution obtained in S2, stirring at 1000-2000 r / min for 30-60 min to completely dissolve it, to obtain a composite inhibitor solution.
[0021] Furthermore, it also includes: after completing step S3, adding a composite inhibitor solution during the blast furnace gravity ash slurry separation process, the amount of the composite inhibitor solution is 1% to 30% by mass in the flotation agent, and then flotation, gravity separation, or magnetic separation is performed.
[0022] Furthermore, the method specifically includes the following steps:
[0023] A: Add 0.1-100 parts by weight of an inorganic inhibitor into 10-100 parts by weight of deionized water, and stir at 1000-2000 r / min for 30-60 minutes to fully dissolve it;
[0024] B: adding 0.1 to 100 parts by weight of an organic inhibitor to the solution prepared in A and stirring at 1000 to 2000 r / min for 30 to 60 min to fully dissolve the organic inhibitor to obtain a mixed solution with a mass fraction of 0.5% to 70%;
[0025] C: Add the prepared composite depressant and flotation agent into the slurry of blast furnace gravity dust removal ash, the amount of which is 1% to 30% by mass in the flotation agent, and then carry out flotation, gravity separation and magnetic separation to obtain carbon powder and iron concentrate products respectively.
[0026] Furthermore, the phosphates include: one or more of sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate.
[0027] Furthermore, the starch includes one or more of corn starch, oxidized starch, pregelatinized starch, and modified starch.
[0028] The addition of the calcium and silicon composite inhibitor of the present invention does not affect the change of the original sorting process, and does not require additional equipment, and can effectively improve the grade of the blast furnace gravity dust removal ash sorting products, namely, iron ore concentrate and carbon powder, reduce the ash content of the carbon powder, increase the calorific value, and effectively increase the economic benefits of the enterprise. The present invention can increase the calorific value of the carbon powder of the blast furnace gravity dust removal ash from 5760 kcal before adding the composite inhibitor of the present invention to 6554 kcal, reduce the ash content of the carbon powder from 25% to 16.99%, and reduce the volatile matter of the carbon powder from 3% to 1.08%. DETAILED DESCRIPTION
[0029] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the present invention is now described.
[0030] The applicant analyzed the existing technology and found that the existing technology did not inhibit calcium and silicon minerals, resulting in a high calcium and silicon content in the product. For example, the presence of calcium and silicon minerals in carbon powder leads to a decrease in the calorific value of the carbon powder, as well as a higher ash content. The calcium and silicon minerals in iron ore concentrate cause a decrease in the grade of total iron, affecting the subsequent sintering ingredients. The presence of calcium and silicon minerals in zinc makes subsequent deep processing and purification difficult.
[0031] Based on the above analysis, the present invention provides a calcium and silicon mineral composite inhibitor for blast furnace gravity dust separation, and the mineral composite inhibitor comprises, by weight:
[0032] 10-100 parts of deionized water, 0.1-100 parts of inorganic inhibitors, 0.1-100 parts of organic inhibitors. The calcium and silicon minerals in blast furnace dust are mainly gangue minerals such as calcium feldspar, mica, calcite, quartz, silicate, etc. Inorganic inhibitors have an effect on gangue minerals such as water glass to generate HSiO3 in the flotation system. - and H2SiO3 on the surface of gangue minerals; sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate are pre-adsorbed on the surface of gangue minerals such as muscovite, quartz and feldspar in the form of phosphate colloid, which weakens the adsorption of collectors on the surface of gangue minerals and increases the hydrophilicity of gangue, thereby inhibiting it. The inhibition of calcite is to make the Ca on the surface of calcite 2+ From the solid phase to the liquid phase, the active sites of the collector adsorption on the calcite surface are reduced, thereby achieving the inhibition of calcite in the blast furnace dust flotation system. Sodium hexametaphosphate has a certain chelating effect and can react with Ca 2+ Mg 2+It can form complexes with other multivalent metal ions, thereby inhibiting minerals containing these ions, and can be used as inhibitors for gangue minerals such as calcite and feldspar. Organic inhibitors such as phenolic hydroxyl groups in the tannin structure can act on the surface of quartz / feldspar through chemical and physical adsorption to form a strong hydrophilic film, and can also cover the hydrophobic layer of the collector on the surface of quartz / feldspar, so that it is strongly inhibited; lignin derivatives have the dual effects of dispersing sludge and inhibiting gangue, which can enhance the effect of collectors and blast furnace dust removal ash, and can also effectively inhibit silicate minerals. Organic colloids, such as carboxymethyl cellulose and starch, are dispersed in water into many molecules of hydrophilic colloid particles, which can be adsorbed on the surface of gangue minerals such as feldspar and calcite to inhibit them. Tartaric acid and oxalic acid molecules are organic molecules with carboxyl groups (-COOH). The carboxyl groups in oxalic acid can form complexes with metal ions through coordination. Tartaric acid and oxalic acid are easily soluble in water and can form complexes of different forms in aqueous solutions. They have strong selectivity and can specifically inhibit the active centers on the surface of gangue minerals, hindering their adsorption with flotation agents. This determines their dissolution behavior and mechanism of action in flotation. Through the combination of inorganic and organic inhibitors, different minerals can be inhibited in the ash separation of blast furnace gravity dust removal, that is, adsorption on the surface of calcium and silicon minerals, increasing hydrophilicity, promoting the surface Ca2+ from the solid phase into the liquid phase, and chelating Ca 2+ Mg 2+ The synergistic effect of forming complexes with other multivalent metal ions effectively improves the efficiency of sorting. By inhibiting calcium and silicon minerals, it effectively prevents them from adhering to the surface of carbon powder, thereby effectively improving the grade of carbon powder. As the fixed carbon of carbon powder increases and impurities decrease, the ash content of carbon powder decreases, and the calorific value increases effectively. Because calcium and silicon minerals are not magnetic and are lighter than iron concentrate, the grade of iron concentrate is improved after magnetic separation and gravity separation, while calcium and silicon minerals enter the tailings after sorting.
[0033] The composite inhibitor of the present invention is added during the slurry separation process of blast furnace gravity ash, and flotation, gravity separation and magnetic separation are carried out normally according to the production process. The present invention can effectively improve the grade of blast furnace gravity dust removal ash separation products, namely iron ore concentrate and carbon powder, reduce the ash content of carbon powder, and increase the calorific value. The grade of iron ore concentrate can be increased by 4% to 15%, or even higher; the grade of carbon powder can be increased by 3% to 12%, or even higher.
[0034] Furthermore, the inorganic inhibitor includes one or more of water glass, sodium carbonate, sodium bicarbonate and phosphates.
[0035] Furthermore, the modulus of the water glass is 2.2-3.0. If the modulus is too small, its inhibition and dispersion effects are weak; if the modulus is too large, its water solubility is small.
[0036] Furthermore, the organic inhibitor includes one or more of tannin, lignin sulfonate, amino enzymatic lignin, tartaric acid, oxalic acid, carboxymethyl cellulose and starch.
[0037] The present invention also provides a method for preparing a composite inhibitor of calcium and silicon minerals for separation of blast furnace gravity dust removal ash, comprising the following steps:
[0038] Step S1: weighing a certain amount of deionized water;
[0039] Step S2: weigh a certain amount of inorganic inhibitor, add it into the deionized water in step S1, stir it at 1000-2000 r / min for 30-60 min to completely dissolve it, and obtain an inorganic inhibitor solution;
[0040] Step S3: weigh a certain amount of organic inhibitor, and add it into the inorganic inhibitor solution obtained in S2, stirring at 1000-2000 r / min for 30-60 min to completely dissolve it, to obtain a composite inhibitor solution.
[0041] Furthermore, it also includes: after completing step S3, adding a composite inhibitor solution during the blast furnace gravity ash slurry separation process, the amount of the composite inhibitor solution is 1% to 30% by mass in the flotation agent, and then flotation, gravity separation, or magnetic separation is performed.
[0042] Furthermore, the method specifically includes the following steps:
[0043] A: Add 0.1-100 parts by weight of an inorganic inhibitor into 10-100 parts by weight of deionized water, and stir at 1000-2000 r / min for 30-60 minutes to fully dissolve it;
[0044] B: adding 0.1 to 100 parts by weight of an organic inhibitor to the solution prepared in A and stirring at 1000 to 2000 r / min for 30 to 60 min to fully dissolve the organic inhibitor to obtain a mixed solution with a mass fraction of 0.5% to 70%;
[0045] C: Add the prepared composite depressant and flotation agent into the slurry of blast furnace gravity dust removal ash, the amount of which is 1% to 30% by mass in the flotation agent, and then carry out flotation, gravity separation and magnetic separation to obtain carbon powder and iron concentrate products respectively.
[0046] Furthermore, the phosphates include: one or more of sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate.
[0047] Furthermore, the starch includes one or more of corn starch, oxidized starch, pregelatinized starch, and modified starch.
[0048] Example 1
[0049] A calcium and silicon mineral composite inhibitor for blast furnace gravity dust separation and a preparation method thereof, comprising the following steps:
[0050] (1) adding 40 parts by weight of inorganic inhibitor sodium hexametaphosphate into 60 parts by weight of deionized water, and stirring at 1000-2000 r / min for 60 minutes to fully dissolve it;
[0051] (2) adding 12 parts by weight of organic inhibitor tannin to the solution prepared in (1) and stirring at 1000-2000 r / min for 30-60 min to fully dissolve the organic inhibitor tannin to obtain an inhibitor mixed solution having a mass fraction of sodium hexametaphosphate of 35.71% and a mass fraction of tannin of 10.71%;
[0052] (3) The prepared composite depressant and flotation agent are added to the slurry of blast furnace gravity dust removal ash, and the amount is adjusted according to the mass percentage of 2% added to the flotation agent, and then flotation, gravity separation and magnetic separation are carried out to obtain carbon powder and iron concentrate products respectively.
[0053] Example 2
[0054] A calcium and silicon mineral composite inhibitor for blast furnace gravity dust separation and a preparation method thereof, comprising the following steps:
[0055] (1) adding 20 parts by weight of sodium water glass with an inorganic inhibitor modulus of 2.5 into 50 parts by weight of deionized water, and stirring at 1000-2000 r / min for 60 minutes to fully dissolve it;
[0056] (2) adding 30 parts by weight of an organic inhibitor sodium lignin sulfonate to the solution prepared in (1) and stirring at 1000-2000 r / min for 30-60 min to fully dissolve the organic inhibitor mixed solution, wherein the mass fraction of sodium water glass is 20% and the mass fraction of sodium lignin sulfonate is 30%;
[0057] (3) The prepared composite depressant and flotation agent are added to the slurry of blast furnace gravity dust removal ash, and the amount is 10% by weight in the flotation agent, and then flotation, gravity separation and magnetic separation are carried out to obtain carbon powder and iron concentrate products respectively.
[0058] Example 3
[0059] A calcium and silicon mineral composite inhibitor for blast furnace gravity dust separation and a preparation method thereof, comprising the following steps:
[0060] (1) adding 30 parts by weight of inorganic inhibitor sodium hexametaphosphate into 30 parts by weight of deionized water, stirring at 1000-2000 r / min for 60 min to fully dissolve it;
[0061] (2) adding 40 parts by weight of an organic inhibitor oxalic acid to the solution prepared in (1), heating the solution to a constant temperature of 60° C., and stirring at 1000 to 2000 r / min for 30 to 60 min to fully dissolve the solution to obtain an inhibitor mixed solution with a mass fraction of 30% sodium hexametaphosphate and a mass fraction of 40% oxalic acid;
[0062] (3) The prepared composite depressant and flotation agent are added to the slurry of blast furnace gravity dust removal ash, and the amount is 8% by weight in the flotation agent, and then flotation, gravity separation and magnetic separation are carried out to obtain carbon powder and iron concentrate products respectively.
[0063] Example 4
[0064] A calcium and silicon mineral composite inhibitor for blast furnace gravity dust separation and a preparation method thereof, comprising the following steps:
[0065] (1) adding 10 parts by weight of inorganic inhibitor sodium phosphate into 85 parts by weight of deionized water, stirring at 1000-2000 r / min for 60 minutes to fully dissolve it;
[0066] (2) adding 5 parts by weight of organic inhibitor carboxymethyl cellulose to the solution prepared in (1) while stirring at a stirring speed of 1000 to 2000 r / min for 30 to 60 minutes to fully dissolve the inhibitor to obtain an inhibitor mixed solution with a mass fraction of sodium phosphate of 10% and a mass fraction of carboxymethyl cellulose of 5%;
[0067] (3) The prepared composite depressant and flotation agent are added to the slurry of blast furnace gravity dust removal ash, and the amount is adjusted according to the mass ratio of the added flotation agent to 20%, and then flotation, gravity separation and magnetic separation are carried out to obtain carbon powder and iron concentrate products respectively.
[0068] Experimental data
[0069] Table 2 Effects of the embodiments of the present invention and the comparative examples on carbon powder indicators
[0070]
[0071]
[0072] Table 3 Effect of the embodiments of the present invention and the comparative examples on the grade index of iron ore concentrate
[0073] Serial number Addition amount % (mass proportion of flotation agent) Total iron grade of iron concentrate (%) Comparison group 0 52% Example 1 2% 56% Example 2 10% 62% Example 3 8% 59% Example 4 20% 65%
[0074] In the above examples, if the specific conditions are not specified, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0075] According to the data in Table 2 and Table 3, it can be seen that the present invention can increase the calorific value of carbon powder in blast furnace gravity dust removal ash from 5760 kcal before adding the composite inhibitor of the present invention to 6554 kcal, reduce the ash content of carbon powder from 25% to 16.99%, reduce the volatile matter of carbon powder from 3% to 1.08%, and increase the total iron grade of iron ore concentrate from 52% to 65%.
[0076] The above description is only an illustrative embodiment of the present invention and is not intended to limit the scope of the present invention. The components of the present invention can be combined with each other without conflict, and any equivalent changes and modifications made by any technician in the field without departing from the concept and principle of the present invention should fall within the scope of protection of the present invention.
Claims
1. A calcium and silicon mineral composite inhibitor for blast furnace gravity dust separation, characterized in that: The mineral composite inhibitor comprises by weight: 10-100 parts of deionized water, 0.1-100 parts of inorganic inhibitors, 0.1-100 parts of organic inhibitors.
2. The mineral composite inhibitor according to claim 1, characterized in that: The inorganic inhibitor includes one or more of water glass, sodium carbonate, sodium bicarbonate and phosphates.
3. The mineral composite inhibitor according to claim 2, characterized in that: The water glass modulus is 2.2-3.
0.
4. The mineral composite inhibitor according to claim 1, characterized in that: The organic inhibitor includes one or more of tannin, lignin sulfonate, amino enzymatic lignin, tartaric acid, oxalic acid, carboxymethyl cellulose and starch.
5. A method for preparing a calcium and silicon mineral composite inhibitor for blast furnace gravity dust separation, characterized in that: The following steps are involved: Step S1: weighing a certain amount of deionized water; Step S2: weigh a certain amount of inorganic inhibitor, add it into the deionized water in step S1, stir it at 1000-2000 r / min for 30-60 min to completely dissolve it, and obtain an inorganic inhibitor solution; Step S3: weigh a certain amount of organic inhibitor, and add it into the inorganic inhibitor solution obtained in S2, stirring at 1000-2000 r / min for 30-60 min to completely dissolve it, to obtain a composite inhibitor solution.
6. The preparation method according to claim 5, characterized in that: Also includes: After completing step S3, a composite inhibitor solution is added during the blast furnace gravity ash slurry separation process, and the amount of the composite inhibitor solution is 1% to 30% by mass in the flotation reagent, and then flotation, gravity separation, or magnetic separation is performed.
7. The preparation method according to claim 5, characterized in that: The specific steps include: A: Add 0.1-100 parts by weight of an inorganic inhibitor into 10-100 parts by weight of deionized water, and stir at 1000-2000 r / min for 30-60 minutes to fully dissolve it; B: adding 0.1 to 100 parts by weight of an organic inhibitor to the solution prepared in A and stirring at 1000 to 2000 r / min for 30 to 60 min to fully dissolve the organic inhibitor to obtain a mixed solution with a mass fraction of 0.5% to 70%; C: Add the prepared composite depressant and flotation agent into the slurry of blast furnace gravity dust removal ash, the amount of which is 1% to 30% by mass in the flotation agent, and then carry out flotation, gravity separation and magnetic separation to obtain carbon powder and iron concentrate products respectively.
8. The preparation method according to claim 5, characterized in that: The phosphates include one or more of sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate.
9. The preparation method according to claim 5, characterized in that: The starch includes one or more of corn starch, oxidized starch, pregelatinized starch and modified starch.
10. The preparation method according to claim 6, characterized in that: The specific steps include: A. Add 10 parts by weight of inorganic inhibitor sodium phosphate into 85 parts by weight of deionized water, and stir at 1000-2000 r / min for 60 minutes to fully dissolve it; B. Add 5 parts by weight of organic inhibitor carboxymethyl cellulose to the solution prepared in step A while stirring at a stirring speed of 1000-2000 r / min, and stir for 30-60 minutes to fully dissolve it, so that the mass fraction of sodium phosphate is 10% and the mass fraction of carboxymethyl cellulose is 5%; obtain a mixed solution of composite inhibitor; C. Add the prepared composite depressant and flotation agent into the slurry of blast furnace gravity dust removal ash, with the amount added according to 20% of the mass in the flotation agent, and then carry out flotation, gravity separation and magnetic separation to obtain carbon powder and iron concentrate products respectively.
Citation Information
Patent Citations
Process for recovering iron and carbon elements from blast furnace gas ash
CN102319617A
Method for recovering zinc, iron and / or carbon from blast furnace gas ash
CN110433956A
Method for recovering carbon, iron and zinc from blast furnace gas dust
CN110813521A