Material production method for reducing surface wrinkles of ferritic stainless steel in stamping and stretching process

By optimizing chemical composition, controlling solidification structure and low-temperature hot rolling process, the problem of surface wrinkles during stamping and stretching of ferrite stainless steel is solved, which significantly improves product quality and pass rate, reduces production costs, and supports its widespread application.

CN119016692APending Publication Date: 2024-11-26SHANXI TAIGANG STAINLESS STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411146579.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The surface of ferrite stainless steel is prone to wrinkles during stamping and stretching, which affects the appearance quality and performance of the product, and it is difficult for the prior art to effectively solve this problem.

Method used

By optimizing the chemical composition of ferrite stainless steel, controlling the solidification structure of continuous casting billets, adopting low-temperature hot rolling process and strictly controlling the temperature gradient and cooling speed during the annealing of cold-rolled finished products, adjusting the microstructure structure of the raw materials and reducing the stamping and stretching process wrinkle in the surface.

Benefits of technology

Effectively reduce the surface wrinkle rate during stamping and stretching, from 8% to below 2%, improve product quality and qualification rate, reduce production costs, and support the widespread application of ferrite stainless steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The ferritic stainless steel is widely applied to industrial production due to excellent corrosion resistance, high strength and good processability. However, in the stamping and stretching process, the surface of the ferritic stainless steel is prone to wrinkling, and the appearance quality and the use performance of the product are seriously affected. Therefore, how to reduce or eliminate the surface wrinkling problem of the ferritic stainless steel in the stamping and stretching process is a research hot spot and difficulty in the field all the time. The invention aims to provide a raw material production method for reducing surface wrinkles in the stamping and stretching process of ferritic stainless steel. According to the method, the microstructure of the raw material is adjusted by optimizing the production process and parameters, so that the surface wrinkling phenomenon in the stamping and stretching process is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of metallurgy and stainless steel production, and in particular to a material production method for reducing surface wrinkling in a ferritic stainless steel stamping and stretching process. Background Art

[0002] Ferritic stainless steel has been widely used in industrial production due to its excellent corrosion resistance, high strength and good processing performance. However, during the stamping and stretching process, the surface of ferritic stainless steel is prone to wrinkling, which seriously affects the appearance quality and performance of the product. Therefore, how to reduce or eliminate the surface wrinkling problem of ferritic stainless steel during the stamping and stretching process has always been a research hotspot and difficulty in this field.

[0003] The present invention aims to provide a raw material production method for reducing surface wrinkling of ferritic stainless steel during stamping and stretching. The method optimizes production process and parameters and adjusts the microstructure of the raw material, thereby effectively reducing the surface wrinkling phenomenon during stamping and stretching. Summary of the invention

[0004] The purpose of the present invention is to address the above-mentioned problems and provide a material production method for reducing surface wrinkling of ferritic stainless steel during stamping and stretching.

[0005] The object of the present invention is achieved by: a material production method for reducing surface wrinkling of ferritic stainless steel during stamping and stretching, comprising the following steps: Step 1: Optimizing and adjusting the chemical composition: C: 0.010-0.025%, Si: 0.20-0.40%, Mn: 0.25- 0.50%, P: ≤0.03%, S: ≤0.005%, Cr: 16.0-16.3%, N: ≤0.03%, Ti: 0.001-0.003%; Step 2: Control the solidification structure of the continuous casting billet: the proportion of equiaxed crystals is between 50-55%, the electromagnetic stirring current is 1350-1600A, the stirring frequency is 2.0-4.0HZ, and the electromagnetic stirring reversing time is 10-30 seconds; Step 3: Use low-temperature hot rolling process: the heating temperature of the casting billet is controlled at 1120-1160℃, the rough rolling outlet temperature RDT1000±20℃, and the finishing rolling outlet temperature FDT900±20℃; Step 4: Control the temperature gradient and cooling rate during the annealing process of the cold-rolled finished product: the heating furnace temperature control mode is the furnace temperature control mode, the furnace temperature is controlled at 840-870℃, the cooling stage is air cooling, and the cooling stage 2 is spray cooling.

[0006] The cooling pressure of the cooling section in step 4 is 1-3 Kg / cm 2 , air volume is 100-150m 3 / min, the spray cooling pressure of the second cooling stage is 6-8Kg / cm 2 , cooling flow rate is 30-60m3 / min, and the cooling speed is 45-60 m / min.

[0007] The beneficial effect of the present invention is that the surface wrinkling phenomenon of the ferritic stainless steel raw material produced by the method of the present invention is significantly reduced during the stamping and stretching process, and the product quality is significantly improved. The surface wrinkling rate during the stamping and stretching process is reduced from 8% to less than 2%. Compared with the traditional method, the present invention not only improves the product qualification rate and reduces the production cost, but also provides strong support for the wide application of ferritic stainless steel. DETAILED DESCRIPTION

[0008] Ferritic stainless steel has been widely used in industrial production due to its excellent corrosion resistance, high strength and good processing performance. However, during the stamping and stretching process, wrinkling easily occurs on the surface of ferritic stainless steel, which seriously affects the appearance quality and performance of the product. Therefore, how to reduce or eliminate the problem of surface wrinkling of ferritic stainless steel during the stamping and stretching process has always been a research hotspot and difficulty in this field. The present invention aims to provide a raw material production method for reducing surface wrinkling of ferritic stainless steel during the stamping and stretching process. The method optimizes the production process and parameters and adjusts the microstructure of the raw materials, thereby effectively reducing the surface wrinkling phenomenon during the stamping and stretching process. The surface wrinkling rate during the stamping and stretching process is reduced from 8% to below 2%.

[0009] The present invention adopts the following technical solutions: 1. Optimize and adjust the chemical composition. Optimize the chemical composition of ferritic stainless steel, reduce the carbon and nitrogen content in the steel, and reduce the performance defects caused by interstitial elements carbon and nitrogen. At the same time, by adding an appropriate amount of alloying element Ti, the toughness and plasticity of stainless steel are improved. Ti and C (carbon) in steel can form very stable TiC. This stable TiC particle helps to refine austenite grains, increase the chance of new phase nucleus formation, and thus accelerate austenite transformation. At the same time, this stable carbide TiC can reduce the harmful effects of carbon, thereby improving the steel's resistance to intergranular corrosion and wrinkling.

[0010]

[0011] 2. Control the solidification structure of the continuous casting billet, and the proportion of equiaxed crystals is greater than 50%. Through electromagnetic stirring technology, the transformation of columnar crystals to equiaxed crystals is promoted, and the solidification structure is refined. At the same time, the electromagnetic force and impact force are used to generate vibration, break the first crystallized dendrites, form more crystal cores, and thus refine the solidification structure. General electromagnetic stirring current: 1350-1600A, stirring frequency: 2.0-4.0HZ, electromagnetic stirring reversing time: 10-30 seconds.

[0012] 3. Use low temperature hot rolling process. The heating temperature of the ingot is generally controlled at 1120-1160℃, the rough rolling outlet temperature is RDT1000±20℃, and the finishing rolling outlet temperature is FDT900±20℃. Low temperature hot rolling can significantly refine the hot rolling structure, strengthen the γ fiber texture, and weaken the α fiber texture, which can effectively improve the forming performance of ferritic stainless steel sheets. In addition, low temperature rolling can also reduce the generation of secondary iron oxide scale, thereby improving the surface quality of hot rolled products.

[0013] 4. Strictly control the temperature gradient and cooling rate during the annealing process of cold-rolled finished products. Adjust the heating furnace temperature control mode from plate temperature control to furnace temperature control mode, and control the furnace temperature between 840-870℃, which can effectively avoid the medium-chromium ferritic stainless steel from affecting the plate temperature measurement due to surface roughness, color difference, etc., and the system frequently adjusts the furnace temperature, resulting in large fluctuations in the performance of the entire strip. The cooling stage is air cooling, and the cooling pressure is 1-3 Kg / cm 2 , air volume is 100-150m 3 / min. The second cooling stage was transformed from the original water spray cooling to spray cooling, and the spray cooling pressure was 6-8Kg / cm 2 , cooling flow rate is 30-60m 3 / min. The cooling speed is 45-60 m / min. It can effectively avoid the unstable performance caused by uneven water spray cooling, thereby maintaining the uniformity and stability of the material structure and reducing stamping wrinkles.

[0014] Through the above four steps, the present invention successfully achieves the optimization and adjustment of the microstructure of the ferritic stainless steel raw material, improves its processing performance during the stamping and stretching process, and effectively reduces the occurrence of surface wrinkling. Embodiment 1

[0015] Steel type: SUS430, hot rolled thickness: 3.0mm, finished product thickness 0.7mm.

[0016] 1. The ingredients are designed as shown in the following table.

[0017]

[0018] 2. Electromagnetic stirring is used in continuous casting, with electromagnetic stirring current of 1550A, stirring frequency of 3.0HZ, electromagnetic stirring reversing time of 20 seconds, and the proportion of equiaxed crystals in the ingot reaches 52%.

[0019] 3. Use low temperature hot rolling process. The heating temperature of the ingot is 1150℃, the rough rolling outlet temperature is RDT1010℃, and the finishing rolling outlet temperature is FDT910℃.

[0020] 4. Temperature control mode of cold-rolled finished product annealing heating furnace: furnace temperature control mode, furnace temperature 860℃. The cooling stage is air cooling, and the cooling pressure is 1.5 Kg / cm2 , air volume is 120m 3 / min. The second stage of cooling adopts spray cooling, and the spray cooling pressure is 6.5Kg / cm 2 , cooling flow rate is 50m 3 / min. The cooling speed is 50 m / min. Effect: The surface wrinkling phenomenon of the ferrite stainless steel raw material produced by the method of the present invention is significantly reduced during the stamping and stretching process, and the product quality is significantly improved. The surface wrinkling rate during the stamping and stretching process is 1.2%. Embodiment 2

[0021] Steel type: SUS430, hot rolled thickness: 3.0mm, finished product thickness 0.7mm.

[0022] 1. The ingredients are designed as shown in the following table.

[0023]

[0024] 2. Electromagnetic stirring is used in continuous casting, with electromagnetic stirring current of 1530A, stirring frequency of 2.5HZ, electromagnetic stirring reversing time of 25 seconds, and the proportion of equiaxed crystals in the ingot reaches 51%.

[0025] 3. Use low temperature hot rolling process. The heating temperature of the ingot is 1145℃, the rough rolling outlet temperature is RDT1020℃, and the finishing rolling outlet temperature is FDT915℃.

[0026] 4. Temperature control mode of cold-rolled finished product annealing heating furnace: furnace temperature control mode, furnace temperature 855℃. The cooling stage is air cooling, and the cooling pressure is 2.0 Kg / cm 2 , air volume is 135m 3 / min. The second stage of cooling adopts spray cooling, and the spray cooling pressure is 6.8Kg / cm 2 , cooling flow rate is 55m 3 / min. The cooling speed is 53 m / min. Effect: The surface wrinkling phenomenon of the ferrite stainless steel raw material produced by the method of the present invention is significantly reduced during the stamping and stretching process, and the product quality is significantly improved. The surface wrinkling rate during the stamping and stretching process is 0.9%.

[0027] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.

Claims

1. A material production method for reducing surface wrinkling of ferritic stainless steel during stamping and stretching, characterized in that: The following steps are involved: Step 1: Optimize and adjust the chemical composition: C: 0.010-0.025%, Si: 0.20-0.40%, Mn: 0.25- 0.50%, P: ≤0.03%, S: ≤0.005%, Cr: 16.0-16.3%, N: ≤0.03%, Ti: 0.001-0.003%; Step 2: Control the solidification structure of the continuous casting billet: the equiaxed crystal ratio is between 50-55%, the electromagnetic stirring current is 1350-1600A, the stirring frequency is 2.0-4.0HZ, and the electromagnetic stirring reversing time is 10-30 seconds; Step 3: Use low temperature hot rolling process: the heating temperature of the ingot is controlled at 1120-1160℃, the rough rolling outlet temperature is RDT1000±20℃, and the finishing rolling outlet temperature is FDT900±20℃; Step 4: Control the temperature gradient and cooling rate during the annealing process of the cold-rolled finished product: the temperature control mode of the heating furnace is the furnace temperature control mode, the furnace temperature is controlled at 840-870°C, the first cooling stage is air cooling, and the second cooling stage is spray cooling.

2. The material production method for reducing surface wrinkling of ferritic stainless steel during stamping and stretching according to claim 1, characterized in that: The cooling pressure of the cooling section in step 4 is 1-3 Kg / cm 2 , air volume is 100-150m 3 / min, the spray cooling pressure of the second cooling stage is 6-8Kg / cm 2 , cooling flow rate is 30-60m 3 / min, and the cooling speed is 45-60 m / min.