Production and manufacturing process of composite finned tube

By employing composite continuous casting and micro-arc oxidation technologies, the problem of loose bonding between steel and aluminum composite finned tubes has been solved, enabling efficient and low-cost production, improving the strength and corrosion resistance of composite finned tubes, and extending their service life.

CN119016708APending Publication Date: 2024-11-26GOLDEN DRAGON PRECISE COPPER TUBE GROUP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411147783.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the existing steel-aluminum composite finned tube processing technology, the bond between the base tube and the outer aluminum skin is not tight, resulting in gaps that lead to corrosion and shortened service life.

Method used

The outer metal layer of the finned tube is cast into an integral piece using a composite continuous casting process, resulting in a tight and seamless bond. A ceramic oxide film is then formed on the surface using a micro-arc oxidation device, which improves the bonding strength and corrosion resistance.

Benefits of technology

This achieves a tight bond between the base tube and the outer metal layer, improving the strength and corrosion resistance of the composite finned tube, extending its service life, and reducing production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016708A_ABST
    Figure CN119016708A_ABST
Patent Text Reader

Abstract

The invention discloses a production and manufacturing process of a composite finned tube, which comprises the following steps of: S1, inserting a base tube into a continuous casting die of a casting furnace, and casting an outer-layer metal of the finned tube and an inner-layer base tube of the finned tube into an integrated composite tube through the continuous casting die; s2, the composite pipe formed through continuous casting is cut into the specified size and length; s3, rolling the coating metal material on the outer layer of the composite tube into a plurality of circles of fins through a fin rolling mill, so as to form a composite finned tube; s4, shifting the two ends of the composite finned tube through a finned tube shifting machine; s5, the composite finned tube is subjected to micro-arc oxidation treatment; the method has the advantages that the overall production cost is low, the machining and production efficiency is high, the produced composite finned tube has the advantages of being high in hardness, excellent in abrasion resistance, corrosion resistance and heat stability and not prone to deflection and deformation, the base tube is prevented from being damaged due to erosion of air and fluid, and the service life of the composite finned tube is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite fin tube processing, in particular to a production process for composite fin tubes. Background Art

[0002] As an innovative heat exchange element, finned tubes have unique and efficient heat exchange performance, and play an irreplaceable role in industrial manufacturing, energy engineering, modern agriculture, etc. Its mechanism of action is that the surface is tightly wound around the tube wall in a spiral shape to form a highly expanded fin surface, which greatly increases the heat exchange area per unit volume. This special fin structure allows the fluid to more fully contact the fins and exchange heat when passing through the tube, whether by conduction or convection, significantly improving the overall heat exchange efficiency, reducing energy loss, and providing technical support for energy conservation and consumption reduction. Steel-aluminum composite finned tubes are widely used because of their strength of steel, high heat transfer and corrosion resistance of aluminum. At present, steel-aluminum composite finned tubes on the market mainly use two processing technologies: winding type and sleeve extrusion type. Among them, the extrusion type is to use a base tube to cover the aluminum tube, and then extrusion molding to process the fins. The winding type is to fix the aluminum strip at one end of the steel tube and produce the fins by winding the strips. However, since both production processes are mechanically processed, the base tube and the outer aluminum skin of the steel-aluminum composite fin tube cannot be tightly combined, and a gap is easily generated between the base tube and the outer aluminum skin, which causes the internal base tube to be corroded by air and fluid. At the same time, since aluminum and steel are two different metals, there is a potential difference between the metals. When the two metals are in the same medium, contact with each other will cause local corrosion of the contact parts, leading to corrosion of the components, greatly shortening the service life of the components, and reducing the use effect. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the existing defects and provide a production and manufacturing process for composite fin tubes with low overall production cost and high processing and production efficiency. The base tube of the produced composite fin tube is tightly combined with the outer metal material coated on the outside without gaps, thereby improving the strength and pressure-bearing capacity of the composite fin tube, maintaining the overall rigidity of the element, and preventing deflection and deformation, thereby avoiding damage to the base tube caused by erosion by air and fluid, and increasing the service life of the composite fin tube. The composite fin tube produced by the production and manufacturing process also has high hardness, excellent wear resistance, excellent corrosion resistance and excellent thermal stability, and can effectively solve the problems in the background technology.

[0004] To achieve the above-mentioned object, the present invention provides the following technical solutions: a manufacturing process of a composite finned tube, the process includes a tube continuous casting device, the tube continuous casting device includes a casting furnace, a continuous casting mold is arranged in the casting furnace, the continuous casting mold extends to the outside of the casting furnace and is provided with a cooling crystallizer, a feeding device for conveying a base tube and passing it through the continuous casting mold is also arranged on the outside of the casting furnace, and a traction device is also arranged on the outside of the casting furnace at the discharge of the continuous casting mold; an outer layer of metal melt for coating the outer wall of the base tube is contained in the casting furnace;

[0005] The process includes the following steps:

[0006] S1. Insert the base tube into the continuous casting mold of the casting furnace, and there is a certain distance between the circumferential outer wall of the base tube and the molding cavity in the continuous casting mold. The outer layer of molten metal in the casting furnace flows into the molding cavity of the continuous casting mold and covers the base tube. The outer layer of molten metal in the continuous casting mold is cooled and solidified by a cooling crystallizer and attached to the base tube, thereby obtaining a composite tube; the base tube is continuously conveyed into the continuous casting mold by a feeding device, and the composite tube is pulled by a pulling device, thereby realizing continuous casting of the composite tube;

[0007] S2, cutting the composite pipe formed by continuous casting into a specified length;

[0008] S3, rolling the outer layer of the composite tube coating metal material into a plurality of fins by a fin rolling mill, thereby forming a composite fin tube;

[0009] S4, using a fin tube head-pulling machine to pull the ends of the composite fin tube, and removing the fins from both ends of the composite fin tube according to the required length;

[0010] S5. Cleaning, degreasing and pickling the composite fin tube to remove dirt and oxide layer on the surface of the composite fin tube;

[0011] S6. The composite fin tube is fixed in the electrolytic cell of the micro-arc oxidation device by a fixture, so that the composite fin tube is completely immersed in the electrolyte, and a high voltage pulse is applied to generate micro-arc discharge on the surface of the composite fin tube to induce an oxidation reaction, so that a ceramic oxide film is formed on the surface of the composite fin tube;

[0012] S7. Clean and dry the composite fin tube to remove residual electrolyte on the surface.

[0013] Furthermore, the base tube is a steel tube, and the outer layer of molten metal is molten aluminum.

[0014] Furthermore, after step S1, the composite pipe may be rolled and then cold drawn to adjust its wall thickness and outer diameter.

[0015] Furthermore, the feeding device conveys the substrate pipe at a speed of 100-1500 mm / min.

[0016] Furthermore, an inert gas filling pipe is connected to the end of the base pipe, and inert gas is continuously filled into the base pipe through the inert gas filling pipe during the continuous casting process of the composite pipe.

[0017] Furthermore, the electrolyte in step S6 includes 5-30 g / L of water-soluble phosphate, 5-30 g / L of water-soluble silicate, 1-10 g / L of alkali metal hydroxide, 5-30 g / L of citrate, and 1-20 g / L of borate, and the solvent is deionized water.

[0018] Furthermore, the power source used by the micro-arc oxidation device in step S6 is a DC pulse power source with a current density of 5-15A / dm 2 , frequency is 500HZ, duty cycle is 4%, temperature is controlled at 20-30℃, and constant current micro-arc oxidation time is 10-30min under continuous stirring.

[0019] Furthermore, the tube continuous casting device also includes a melting furnace for melting the outer layer of the composite fin tube cladding metal material into an outer layer metal melt. The melting furnace is connected to the casting furnace through a connecting pipe, and a plug is also provided at the liquid outlet of the melting furnace.

[0020] Furthermore, the continuous casting mold is a hollow tubular structure, and a composite hole is opened at the center of the bottom of the continuous casting mold. The diameter of the composite hole is larger than the hollow hole of the continuous casting mold. The top of the hollow hole of the continuous casting mold is a positioning hole, and the diameter of the positioning hole is adapted to the outer diameter of the base tube; a drainage hole connected to the composite hole is opened on the circumferential side wall of the continuous casting mold.

[0021] Compared with the prior art, the invention has the following beneficial effects: the manufacturing process of the composite finned tube firstly casts the outer metal of the finned tube and the inner base tube of the finned tube into an integrated composite tube through a composite continuous casting process, thereby realizing the continuous production of the long-size composite tube; then, the coated alloy layer material of the composite tube is rolled into a plurality of fins by a fin rolling mill, thereby forming a composite finned tube; finally, the surface of the steel-aluminum composite finned tube is subjected to a micro-arc oxidation reaction by a micro-arc oxidation device, thereby forming a ceramic oxide film on the surface of the steel-aluminum composite finned tube; the ... The overall production cost of the composite fin tube production process is low, and the processing and production efficiency is high. The base tube of the composite fin tube produced is tightly combined with the outer metal material coated on the outside without gaps, thereby improving the strength and pressure bearing capacity of the composite fin tube, maintaining the overall rigidity of the component, and preventing deflection and deformation, thereby avoiding damage to the base tube caused by erosion by air and fluid, and increasing the service life of the composite fin tube. The composite fin tube produced by this production process also has high hardness, excellent wear resistance, excellent corrosion resistance and excellent thermal stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic structural diagram of the pipe continuous casting device of the present invention;

[0023] Figure 2 This is a schematic diagram of the structure of the pipe casting mold of the present invention;

[0024] Figure 3 The working condition diagram of the gap between the steel layer and the aluminum layer of the steel-aluminum composite fin tube manufactured by the steel-aluminum composite fin tube production process of the present invention is observed by a 50x microscope;

[0025] Figure 4 The working condition diagram of the bonding surface area of ​​the steel layer and the aluminum layer of the steel-aluminum composite fin tube manufactured by the steel-aluminum composite fin tube production process of the present invention after the corrosion test is observed by using a 100-fold microscope;

[0026] Figure 5 This is a working diagram of the gap between the steel layer and the aluminum layer of the steel-aluminum composite fin tube manufactured by the traditional sleeve extrusion production process, observed using a 50x microscope;

[0027] Figure 6 A 100x microscope was used to observe the working condition of the steel layer and aluminum layer interface area of ​​the steel-aluminum composite fin tube manufactured by the traditional sleeve extrusion production process after the corrosion test.

[0028] In the figure: 1. base pipe; 2. melting furnace; 3. casting furnace; 4. continuous casting mold; 41. positioning hole; 42. composite hole; 43. drainage hole; 5. connecting pipeline; 6. composite pipe; 7. feeding device; 8. traction device; 9. plug; 10. inert gas filling pipe. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] See also Figure 1-2 The present invention provides a technical solution: a production process of a composite finned tube, the process includes a tube continuous casting device, the tube continuous casting device includes a casting furnace 3, a continuous casting mold 4 is arranged in the casting furnace 3, the continuous casting mold 4 is a hollow tubular structure, a composite hole 42 is opened at the center of the bottom of the continuous casting mold 4, the diameter of the composite hole 42 is larger than the hollow hole of the continuous casting mold 4, the top of the hollow hole of the continuous casting mold 4 is a positioning hole 41, and the diameter of the positioning hole 41 is adapted to the outer diameter of the base tube 1; a drainage hole 43 connected with the composite hole 42 is opened on the circumferential side wall of the continuous casting mold 4; the continuous casting mold 4 extends to the outside of the casting furnace 3 and is provided with a cooling crystallizer; the casting furnace 3 contains an outer layer of molten metal for coating the outer wall of the base tube 1;

[0032] The tube continuous casting device also includes a melting furnace 2 for melting the outer layer of the composite fin tube into an outer layer of molten metal. The melting furnace 2 is connected to the casting furnace 3 through a connecting pipe 5, and a plug 9 is provided at the liquid outlet of the melting furnace 2; a feeding device 7 for conveying the base tube 1 and passing it through the continuous casting mold 4 is provided on the outside of the casting furnace 3, and a traction device 8 is provided on the outside of the casting furnace 3 at the discharge of the continuous casting mold 4; the base tube 1 is a steel tube, and the outer layer of molten metal is aluminum liquid.

[0033] The process includes the following steps:

[0034] S1. Insert the base tube 1 into the continuous casting mold 4 of the casting furnace 3, position the base tube 1 through the positioning hole 41, and there is a certain distance between the circumferential outer wall of the base tube 1 and the composite hole 42 in the continuous casting mold 4. The aluminum liquid in the melting furnace 2 flows into the casting furnace 3 through the connecting pipe 5, and the aluminum liquid in the casting furnace 3 flows into the composite hole 42 of the continuous casting mold 4 through the drainage hole 43 and covers the base tube 1. The aluminum liquid in the continuous casting mold 4 is cooled and solidified by the cooling crystallizer and attached to the base tube 1, thereby obtaining to the composite pipe 6, i.e., the steel-aluminum composite pipe; the base pipe 1 is continuously conveyed into the continuous casting mold 4 by the feeding device 7, and the composite pipe 6 is pulled by the pulling device 8, so as to realize the continuous casting of the composite pipe 6; the end of the base pipe 1 is connected with an inert gas filling pipe 10, and inert gas is continuously filled into the base pipe 1 through the inert gas filling pipe 10 during the continuous casting process of the composite pipe 6, so as to protect the inner wall of the base pipe 1 from oxidation and avoid oxidation and decarburization of the inner wall of the base pipe 1;

[0035] S2, cutting the continuously cast composite pipe 6 into a specified length;

[0036] S3, rolling the outer layer of the composite tube 6 into a plurality of fins by a fin rolling mill, thereby forming a steel-aluminum composite fin tube;

[0037] S4, use a fin tube head-pulling machine to pull the ends of the steel-aluminum composite fin tube and remove the fins at both ends of the steel-aluminum composite fin tube according to the required length;

[0038] S5. Clean, degrease and pickle the steel-aluminum composite fin tube to remove dirt and oxide layer on the surface of the steel-aluminum composite fin tube;

[0039] S6. The steel-aluminum composite fin tube is fixed in the electrolytic cell of the micro-arc oxidation device by a fixture, so that the steel-aluminum composite fin tube is completely immersed in the electrolyte, and a high voltage pulse is applied to generate a micro-arc discharge on the surface of the steel-aluminum composite fin tube to induce an oxidation reaction, so that a ceramic oxide film is formed on the surface of the steel-aluminum composite fin tube; the electrolyte includes 15g / L sodium phosphate, 9g / L sodium silicate, 8g / L sodium hydroxide, 14g / L sodium citrate, 8g / L sodium borate, and the balance is deionized water; the power supply used by the micro-arc oxidation device is a DC pulse power supply with a current density of 10A / dm 2 , frequency is 500HZ, duty cycle is 4%, temperature is 25℃, and constant current micro-arc oxidation time is 15min under continuous stirring.

[0040] S7. Clean and dry the steel-aluminum composite fin tube to remove residual electrolyte on the surface.

[0041] Furthermore, after step S1, the composite tube 6 may be rolled and then cold drawn to adjust its wall thickness and outer diameter.

[0042] Furthermore, the feeding device 7 conveys the substrate tube 1 at a speed of 100 mm / min.

[0043] The sodium phosphate used in this embodiment can be replaced by other water-soluble phosphates, such as sodium dihydrogen phosphate or disodium hydrogen phosphate; sodium silicate can be replaced by other water-soluble silicates, such as potassium silicate or lithium silicate; sodium hydroxide can be replaced by other alkali metal hydroxides, such as potassium hydroxide or barium hydroxide; sodium citrate can be replaced by other citrates, such as potassium citrate; sodium borate can be replaced by other borates, such as zinc borate.

[0044] Example 2

[0045] See also Figure 1-2 The present invention also provides a technical solution: a production process of a composite finned tube, the process includes a tube continuous casting device, the tube continuous casting device includes a casting furnace 3, a continuous casting mold 4 is arranged in the casting furnace 3, the continuous casting mold 4 is a hollow tubular structure, a composite hole 42 is opened at the center of the bottom of the continuous casting mold 4, the diameter of the composite hole 42 is larger than the hollow hole of the continuous casting mold 4, the top of the hollow hole of the continuous casting mold 4 is a positioning hole 41, and the diameter of the positioning hole 41 is adapted to the outer diameter of the base tube 1; a drainage hole 43 connected to the composite hole 42 is opened on the circumferential side wall of the continuous casting mold 4; the continuous casting mold 4 extends to the outside of the casting furnace 3 and is provided with a cooling crystallizer; the casting furnace 3 contains an outer layer of molten metal for coating the outer wall of the base tube 1;

[0046] The tube continuous casting device also includes a melting furnace 2 for melting the outer layer of the composite fin tube into an outer layer of molten metal. The melting furnace 2 is connected to the casting furnace 3 through a connecting pipe 5, and a plug 9 is provided at the liquid outlet of the melting furnace 2; a feeding device 7 for conveying the base tube 1 and passing it through the continuous casting mold 4 is provided on the outside of the casting furnace 3, and a traction device 8 is provided on the outside of the casting furnace 3 at the discharge of the continuous casting mold 4; the base tube 1 is a steel tube, and the outer layer of molten metal is aluminum liquid.

[0047] The process includes the following steps:

[0048] S1. Insert the base tube 1 into the continuous casting mold 4 of the casting furnace 3, position the base tube 1 through the positioning hole 41, and there is a certain distance between the circumferential outer wall of the base tube 1 and the composite hole 42 in the continuous casting mold 4. The aluminum liquid in the melting furnace 2 flows into the casting furnace 3 through the connecting pipe 5, and the aluminum liquid in the casting furnace 3 flows into the composite hole 42 of the continuous casting mold 4 through the drainage hole 43 and covers the base tube 1. The aluminum liquid in the continuous casting mold 4 is cooled and solidified by the cooling crystallizer and attached to the base tube 1, thereby obtaining to the composite pipe 6, i.e., the steel-aluminum composite pipe; the base pipe 1 is continuously conveyed into the continuous casting mold 4 by the feeding device 7, and the composite pipe 6 is pulled by the pulling device 8, so as to realize the continuous casting of the composite pipe 6; the end of the base pipe 1 is connected with an inert gas filling pipe 10, and inert gas is continuously filled into the base pipe 1 through the inert gas filling pipe 10 during the continuous casting process of the composite pipe 6, so as to protect the inner wall of the base pipe 1 from oxidation and avoid oxidation and decarburization of the inner wall of the base pipe 1;

[0049] S2, cutting the continuously cast composite pipe 6 into a specified length;

[0050] S3, rolling the outer layer of the composite tube 6 into a plurality of fins by a fin rolling mill, thereby forming a steel-aluminum composite fin tube;

[0051] S4, use a fin tube head-pulling machine to pull the ends of the steel-aluminum composite fin tube and remove the fins at both ends of the steel-aluminum composite fin tube according to the required length;

[0052] S5. Clean, degrease and pickle the steel-aluminum composite fin tube to remove dirt and oxide layer on the surface of the steel-aluminum composite fin tube;

[0053] S6. The steel-aluminum composite finned tube is fixed in the electrolytic cell of the micro-arc oxidation device by a fixture, so that the steel-aluminum composite finned tube is completely immersed in the electrolyte, and a high voltage pulse is applied to generate a micro-arc discharge on the surface of the steel-aluminum composite finned tube to induce an oxidation reaction, so that a ceramic oxide film is formed on the surface of the steel-aluminum composite finned tube; the electrolyte includes 5g / L sodium phosphate, 5g / L sodium silicate, 1g / L sodium hydroxide, 5g / L sodium citrate, 1g / L sodium borate, and the balance is deionized water; the power supply used by the micro-arc oxidation device is a DC pulse power supply with a current density of 10A / dm 2 , frequency is 500HZ, duty cycle is 4%, temperature is 25℃, and constant current micro-arc oxidation time is 15min under continuous stirring.

[0054] S7. Clean and dry the steel-aluminum composite fin tube to remove residual electrolyte on the surface.

[0055] Furthermore, after step S1, the composite tube 6 may be rolled and then cold drawn to adjust its wall thickness and outer diameter.

[0056] Furthermore, the conveying speed of the feeding device 7 for the substrate tube 1 is 1000 mm / min;

[0057] The sodium phosphate used in this embodiment can be replaced by other water-soluble phosphates, such as sodium dihydrogen phosphate or disodium hydrogen phosphate; sodium silicate can be replaced by other water-soluble silicates, such as potassium silicate or lithium silicate; sodium hydroxide can be replaced by other alkali metal hydroxides, such as potassium hydroxide or barium hydroxide; sodium citrate can be replaced by other citrates, such as potassium citrate; sodium borate can be replaced by other borates, such as zinc borate.

[0058] Example 3

[0059] See also Figure 1-2 The present invention also provides a technical solution: a production process of a composite finned tube, the process includes a tube continuous casting device, the tube continuous casting device includes a casting furnace 3, a continuous casting mold 4 is arranged in the casting furnace 3, the continuous casting mold 4 is a hollow tubular structure, a composite hole 42 is opened at the center of the bottom of the continuous casting mold 4, the diameter of the composite hole 42 is larger than the hollow hole of the continuous casting mold 4, the top of the hollow hole of the continuous casting mold 4 is a positioning hole 41, and the diameter of the positioning hole 41 is adapted to the outer diameter of the base tube 1; a drainage hole 43 connected to the composite hole 42 is opened on the circumferential side wall of the continuous casting mold 4; the continuous casting mold 4 extends to the outside of the casting furnace 3 and is provided with a cooling crystallizer; the casting furnace 3 contains an outer layer of molten metal for coating the outer wall of the base tube 1;

[0060] The tube continuous casting device also includes a melting furnace 2 for melting the outer layer of the composite fin tube into an outer layer of molten metal. The melting furnace 2 is connected to the casting furnace 3 through a connecting pipe 5, and a plug 9 is provided at the liquid outlet of the melting furnace 2; a feeding device 7 for conveying the base tube 1 and passing it through the continuous casting mold 4 is provided on the outside of the casting furnace 3, and a traction device 8 is provided on the outside of the casting furnace 3 at the discharge of the continuous casting mold 4; the base tube 1 is a steel tube, and the outer layer of molten metal is aluminum liquid.

[0061] The process includes the following steps:

[0062] S1. Insert the base tube 1 into the continuous casting mold 4 of the casting furnace 3, position the base tube 1 through the positioning hole 41, and there is a certain distance between the circumferential outer wall of the base tube 1 and the composite hole 42 in the continuous casting mold 4. The aluminum liquid in the melting furnace 2 flows into the casting furnace 3 through the connecting pipe 5, and the aluminum liquid in the casting furnace 3 flows into the composite hole 42 of the continuous casting mold 4 through the drainage hole 43 and covers the base tube 1. The aluminum liquid in the continuous casting mold 4 is cooled and solidified by the cooling crystallizer and attached to the base tube 1, thereby obtaining to the composite pipe 6, i.e., the steel-aluminum composite pipe; the base pipe 1 is continuously conveyed into the continuous casting mold 4 by the feeding device 7, and the composite pipe 6 is pulled by the pulling device 8, so as to realize the continuous casting of the composite pipe 6; the end of the base pipe 1 is connected with an inert gas filling pipe 10, and inert gas is continuously filled into the base pipe 1 through the inert gas filling pipe 10 during the continuous casting process of the composite pipe 6, so as to protect the inner wall of the base pipe 1 from oxidation and avoid oxidation and decarburization of the inner wall of the base pipe 1;

[0063] S2, cutting the continuously cast composite pipe 6 into a specified length;

[0064] S3, rolling the outer layer of the composite tube 6 into a plurality of fins by a fin rolling mill, thereby forming a steel-aluminum composite fin tube;

[0065] S4, use a fin tube head-pulling machine to pull the ends of the steel-aluminum composite fin tube and remove the fins at both ends of the steel-aluminum composite fin tube according to the required length;

[0066] S5. Clean, degrease and pickle the steel-aluminum composite fin tube to remove dirt and oxide layer on the surface of the steel-aluminum composite fin tube;

[0067] S6. The steel-aluminum composite finned tube is fixed in the electrolytic cell of the micro-arc oxidation device by a fixture, so that the steel-aluminum composite finned tube is completely immersed in the electrolyte, and a high voltage pulse is applied to generate a micro-arc discharge on the surface of the steel-aluminum composite finned tube to induce an oxidation reaction, so that a ceramic oxide film is formed on the surface of the steel-aluminum composite finned tube; the electrolyte includes 30g / L sodium phosphate, 30g / L sodium silicate, 10g / L sodium hydroxide, 30g / L sodium citrate, 20g / L sodium borate, and the balance is deionized water; the power supply used by the micro-arc oxidation device is a DC pulse power supply with a current density of 10A / dm 2 , frequency is 500HZ, duty cycle is 4%, temperature is 25℃, and constant current micro-arc oxidation time is 15min under continuous stirring.

[0068] S7. Clean and dry the steel-aluminum composite fin tube to remove residual electrolyte on the surface.

[0069] Furthermore, after step S1, the composite tube 6 may be rolled and then cold drawn to adjust its wall thickness and outer diameter.

[0070] Furthermore, the conveying speed of the feeding device 7 for the substrate tube 1 is 1500 mm / min.

[0071] The sodium phosphate used in this embodiment can be replaced by other water-soluble phosphates, such as sodium dihydrogen phosphate or disodium hydrogen phosphate; sodium silicate can be replaced by other water-soluble silicates, such as potassium silicate or lithium silicate; sodium hydroxide can be replaced by other alkali metal hydroxides, such as potassium hydroxide or barium hydroxide; sodium citrate can be replaced by other citrates, such as potassium citrate; sodium borate can be replaced by other borates, such as zinc borate.

[0072] Example 4

[0073] See also Figure 1-2 The present invention provides a technical solution: a production process of a composite finned tube, the process includes a tube continuous casting device, the tube continuous casting device includes a casting furnace 3, a continuous casting mold 4 is arranged in the casting furnace 3, the continuous casting mold 4 is a hollow tubular structure, a composite hole 42 is opened at the center of the bottom of the continuous casting mold 4, the diameter of the composite hole 42 is larger than the hollow hole of the continuous casting mold 4, the top of the hollow hole of the continuous casting mold 4 is a positioning hole 41, and the diameter of the positioning hole 41 is adapted to the outer diameter of the base tube 1; a drainage hole 43 connected with the composite hole 42 is opened on the circumferential side wall of the continuous casting mold 4; the continuous casting mold 4 extends to the outside of the casting furnace 3 and is provided with a cooling crystallizer; the casting furnace 3 contains an outer layer of molten metal for coating the outer wall of the base tube 1;

[0074] The tube continuous casting device also includes a melting furnace 2 for melting the outer layer of the composite fin tube into an outer layer of molten metal. The melting furnace 2 is connected to the casting furnace 3 through a connecting pipe 5, and a plug 9 is provided at the liquid outlet of the melting furnace 2; a feeding device 7 for conveying the base tube 1 and passing it through the continuous casting mold 4 is provided on the outside of the casting furnace 3, and a traction device 8 is provided on the outside of the casting furnace 3 at the discharge of the continuous casting mold 4; the base tube 1 is a steel tube, and the outer layer of molten metal is aluminum liquid.

[0075] The process includes the following steps:

[0076] S1. Insert the base tube 1 into the continuous casting mold 4 of the casting furnace 3, position the base tube 1 through the positioning hole 41, and there is a certain distance between the circumferential outer wall of the base tube 1 and the composite hole 42 in the continuous casting mold 4. The aluminum liquid in the melting furnace 2 flows into the casting furnace 3 through the connecting pipe 5, and the aluminum liquid in the casting furnace 3 flows into the composite hole 42 of the continuous casting mold 4 through the drainage hole 43 and covers the base tube 1. The aluminum liquid in the continuous casting mold 4 is cooled and solidified by the cooling crystallizer and attached to the base tube 1, thereby obtaining to the composite pipe 6, i.e., the steel-aluminum composite pipe; the base pipe 1 is continuously conveyed into the continuous casting mold 4 by the feeding device 7, and the composite pipe 6 is pulled by the pulling device 8, so as to realize the continuous casting of the composite pipe 6; the end of the base pipe 1 is connected with an inert gas filling pipe 10, and inert gas is continuously filled into the base pipe 1 through the inert gas filling pipe 10 during the continuous casting process of the composite pipe 6, so as to protect the inner wall of the base pipe 1 from oxidation and avoid oxidation and decarburization of the inner wall of the base pipe 1;

[0077] S2, cutting the continuously cast composite pipe 6 into a specified length;

[0078] S3, rolling the outer layer of the composite tube 6 into a plurality of fins by a fin rolling mill, thereby forming a steel-aluminum composite fin tube;

[0079] S4, use a fin tube head-pulling machine to pull the ends of the steel-aluminum composite fin tube and remove the fins at both ends of the steel-aluminum composite fin tube according to the required length;

[0080] S5. Clean, degrease and pickle the steel-aluminum composite fin tube to remove dirt and oxide layer on the surface of the steel-aluminum composite fin tube;

[0081] S6. The steel-aluminum composite finned tube is fixed in the electrolytic cell of the micro-arc oxidation device by a fixture, so that the steel-aluminum composite finned tube is completely immersed in the electrolyte, and a high voltage pulse is applied to generate a micro-arc discharge on the surface of the steel-aluminum composite finned tube to induce an oxidation reaction, so that a ceramic oxide film is formed on the surface of the steel-aluminum composite finned tube; the electrolyte includes 15g / L sodium phosphate, 9g / L sodium silicate, 8g / L sodium hydroxide, 14g / L sodium citrate, 8g / L sodium borate, and the balance is deionized water; the power supply used by the micro-arc oxidation device is a DC pulse power supply with a current density of 5A / dm 2 , frequency is 500HZ, duty cycle is 4%, temperature is 20℃, and constant current micro-arc oxidation time is 10min under continuous stirring.

[0082] S7. Clean and dry the steel-aluminum composite fin tube to remove residual electrolyte on the surface.

[0083] Furthermore, after step S1, the composite tube 6 may be rolled and then cold drawn to adjust its wall thickness and outer diameter.

[0084] Furthermore, the feeding device 7 conveys the substrate tube 1 at a speed of 100 mm / min.

[0085] The sodium phosphate used in this embodiment can be replaced by other water-soluble phosphates, such as sodium dihydrogen phosphate or disodium hydrogen phosphate; sodium silicate can be replaced by other water-soluble silicates, such as potassium silicate or lithium silicate; sodium hydroxide can be replaced by other alkali metal hydroxides, such as potassium hydroxide or barium hydroxide; sodium citrate can be replaced by other citrates, such as potassium citrate; sodium borate can be replaced by other borates, such as zinc borate.

[0086] Example 5

[0087] See also Figure 1-2 The present invention provides a technical solution: a production process of a composite finned tube, the process includes a tube continuous casting device, the tube continuous casting device includes a casting furnace 3, a continuous casting mold 4 is arranged in the casting furnace 3, the continuous casting mold 4 is a hollow tubular structure, a composite hole 42 is opened at the center of the bottom of the continuous casting mold 4, the diameter of the composite hole 42 is larger than the hollow hole of the continuous casting mold 4, the top of the hollow hole of the continuous casting mold 4 is a positioning hole 41, and the diameter of the positioning hole 41 is adapted to the outer diameter of the base tube 1; a drainage hole 43 connected with the composite hole 42 is opened on the circumferential side wall of the continuous casting mold 4; the continuous casting mold 4 extends to the outside of the casting furnace 3 and is provided with a cooling crystallizer; the casting furnace 3 contains an outer layer of molten metal for coating the outer wall of the base tube 1;

[0088] The tube continuous casting device also includes a melting furnace 2 for melting the outer layer of the composite fin tube into an outer layer of molten metal. The melting furnace 2 is connected to the casting furnace 3 through a connecting pipe 5, and a plug 9 is provided at the liquid outlet of the melting furnace 2; a feeding device 7 for conveying the base tube 1 and passing it through the continuous casting mold 4 is provided on the outside of the casting furnace 3, and a traction device 8 is provided on the outside of the casting furnace 3 at the discharge of the continuous casting mold 4; the base tube 1 is a steel tube, and the outer layer of molten metal is aluminum liquid.

[0089] The process includes the following steps:

[0090] S1. Insert the base tube 1 into the continuous casting mold 4 of the casting furnace 3, position the base tube 1 through the positioning hole 41, and there is a certain distance between the circumferential outer wall of the base tube 1 and the composite hole 42 in the continuous casting mold 4. The aluminum liquid in the melting furnace 2 flows into the casting furnace 3 through the connecting pipe 5, and the aluminum liquid in the casting furnace 3 flows into the composite hole 42 of the continuous casting mold 4 through the drainage hole 43 and covers the base tube 1. The aluminum liquid in the continuous casting mold 4 is cooled and solidified by the cooling crystallizer and attached to the base tube 1, thereby obtaining to the composite pipe 6, i.e., the steel-aluminum composite pipe; the base pipe 1 is continuously conveyed into the continuous casting mold 4 by the feeding device 7, and the composite pipe 6 is pulled by the pulling device 8, so as to realize the continuous casting of the composite pipe 6; the end of the base pipe 1 is connected with an inert gas filling pipe 10, and inert gas is continuously filled into the base pipe 1 through the inert gas filling pipe 10 during the continuous casting process of the composite pipe 6, so as to protect the inner wall of the base pipe 1 from oxidation and avoid oxidation and decarburization of the inner wall of the base pipe 1;

[0091] S2, cutting the continuously cast composite pipe 6 into a specified length;

[0092] S3, rolling the outer layer of the composite tube 6 into a plurality of fins by a fin rolling mill, thereby forming a steel-aluminum composite fin tube;

[0093] S4, use a fin tube head-pulling machine to pull the ends of the steel-aluminum composite fin tube and remove the fins at both ends of the steel-aluminum composite fin tube according to the required length;

[0094] S5. Clean, degrease and pickle the steel-aluminum composite fin tube to remove dirt and oxide layer on the surface of the steel-aluminum composite fin tube;

[0095] S6. The steel-aluminum composite fin tube is fixed in the electrolytic cell of the micro-arc oxidation device by a fixture, so that the steel-aluminum composite fin tube is completely immersed in the electrolyte, and a high voltage pulse is applied. Micro-arc discharge is generated on the surface of the steel-aluminum composite fin tube to induce an oxidation reaction, so that a ceramic oxide film is formed on the surface of the steel-aluminum composite fin tube; the electrolyte includes 15g / L sodium phosphate, 9g / L sodium silicate, 8g / L sodium hydroxide, 14g / L sodium citrate, 8g / L sodium borate, and the balance is deionized water; the power supply used by the micro-arc oxidation device is a DC pulse power supply with a current density of 15A / dm 2 , frequency is 500HZ, duty cycle is 4%, temperature is 30℃, and constant current micro-arc oxidation time is 30min under continuous stirring.

[0096] S7. Clean and dry the steel-aluminum composite fin tube to remove residual electrolyte on the surface.

[0097] Furthermore, after step S1, the composite tube 6 may be rolled and then cold drawn to adjust its wall thickness and outer diameter.

[0098] Furthermore, the feeding device 7 conveys the substrate tube 1 at a speed of 100 mm / min.

[0099] The sodium phosphate used in this embodiment can be replaced by other water-soluble phosphates, such as sodium dihydrogen phosphate or disodium hydrogen phosphate; sodium silicate can be replaced by other water-soluble silicates, such as potassium silicate or lithium silicate; sodium hydroxide can be replaced by other alkali metal hydroxides, such as potassium hydroxide or barium hydroxide; sodium citrate can be replaced by other citrates, such as potassium citrate; sodium borate can be replaced by other borates, such as zinc borate.

[0100] Comparative Example 1: Compared with the micro-arc oxidation process in step S6 of the present invention, the electrolyte includes 5 g / L sodium silicate, 1 g / L sodium hydroxide, 5 g / L sodium citrate, 1 g / L sodium borate, and the balance is deionized water; the power supply used in the micro-arc oxidation is a DC pulse power supply with a current density of 10 A / dm 2 , frequency is 500HZ, duty cycle is 4%, temperature is 25℃, and constant current micro-arc oxidation time is 15min under continuous stirring.

[0101] Comparative Example 2: Compared with the micro-arc oxidation process in step S6 of the present invention, the electrolyte includes 15 g / L sodium phosphate, 9 g / L sodium silicate, 14 g / L sodium citrate, 8 g / L sodium borate, and the balance is deionized water; the power supply used in the micro-arc oxidation is a DC pulse power supply with a current density of 10 A / dm 2 , frequency is 500HZ, duty cycle is 4%, temperature is 25℃, and constant current micro-arc oxidation time is 15min under continuous stirring.

[0102] Comparative Example 3: Compared with the micro-arc oxidation processing in step S6 of the present invention, the electrolyte includes 15 g / L sodium phosphate, 9 g / L sodium silicate, 8 g / L sodium hydroxide, 14 g / L sodium citrate, 8 g / L sodium borate, and the balance is deionized water; the micro-arc oxidation device is not powered on, and only the sample is immersed in the electrolyte, the immersion temperature is 25°C, and the oxidation time is 15 minutes under continuous stirring.

[0103] Comparative Example 4: Compared with the micro-arc oxidation process in step S6 of the present invention, the electrolyte includes 15 g / L sodium phosphate, 9 g / L sodium silicate, 8 g / L sodium hydroxide, 14 g / L sodium citrate, 8 g / L sodium borate, and the balance is deionized water; the power supply used for micro-arc oxidation is a DC pulse power supply with a current density of 10 A / dm 2 , frequency is 500HZ, duty cycle is 4%, temperature is 25℃, constant current micro-arc oxidation time is 15min, and no stirring operation is performed during the processing.

[0104] Comparative Example 5: Compared with the micro-arc oxidation process in step S6 of the present invention, the electrolyte includes 4 g / L sodium phosphate, 4 g / L sodium silicate, 0.5 g / L sodium hydroxide, 4 g / L sodium citrate, 0.5 g / L sodium borate, and the balance is deionized water; the power supply used for micro-arc oxidation is a DC pulse power supply with a current density of 10 A / dm 2 , frequency is 500HZ, duty cycle is 4%, temperature is 25℃, and constant current micro-arc oxidation time is 15min under continuous stirring.

[0105] Comparative Example 6: Compared with the micro-arc oxidation process in step S6 of the present invention, the electrolyte includes 40 g / L sodium phosphate, 40 g / L sodium silicate, 15 g / L sodium hydroxide, 40 g / L sodium citrate, 25 g / L sodium borate, and the balance is deionized water; the power supply used in the micro-arc oxidation is a DC pulse power supply with a current density of 10 A / dm 2 , frequency is 500HZ, duty cycle is 4%, temperature is 25℃, and constant current micro-arc oxidation time is 15min under continuous stirring.

[0106] Test verification: The steel-aluminum composite fin tube processed in step S5 of the present invention was subjected to micro-arc oxidation using the electrolytes of Examples 1-5 and Comparative Examples 1-6, respectively, and a comparative analysis was performed using a 500-hour neutral salt spray test method. The test data are shown in Table 1:

[0107] Table 1 Comparative experimental data of different electrolyte compositions on micro-arc oxidation processing of steel-aluminum composite fin tubes

[0108] Grouping Hardness tester to test film hardness 500 hours salt spray test level Example 1 1836HV Level 10 Example 2 1147HV Level 8 Example 3 1335HV Level 9 Example 4 1829HV Level 10 Example 5 1172HV Level 8 Comparative Example 1 324HV Level 5 Comparative Example 2 427HV Level 4 Comparative Example 3 100HV Level 3 Comparative Example 4 1322HV Level 8 Comparative Example 5 543HV Level 8 Comparative Example 6 1794HV Level 10

[0109] It can be seen from Table 1 that after the steel-aluminum composite fin tubes are subjected to micro-arc oxidation processing using the electrolytes of Example 1, Example 2, Example 3, Example 4 and Example 5, the steel-aluminum composite fin tubes have high hardness, high corrosion resistance grade and strong corrosion resistance.

[0110] However, after the steel-aluminum composite fin tubes were subjected to micro-arc oxidation processing using the electrolytes of Comparative Examples 1, 2, 3 and 5, the steel-aluminum composite fin tubes had low hardness, low corrosion resistance grade and poor corrosion resistance.

[0111] In the case where no stirring was performed in Comparative Example 4, the treated steel-aluminum composite fin tube had poorer hardness and corrosion resistance than the treated steel-aluminum composite fin tube in Example 1.

[0112] In Comparative Example 6, when the content levels of all components are significantly higher, the treated steel-aluminum composite fin tube has strong hardness and corrosion resistance, but there are more undissolved components remaining in the electrolyte prepared therefrom, which is an obvious waste from a cost perspective.

[0113] See also Figure 3 The 50x microscope observation shown shows the gap condition between the steel layer and the aluminum layer of the steel-aluminum composite fin tube manufactured by the process of the present invention. It can be seen that there is no gap between the steel layer and the aluminum layer, the composite fin tube is in good cladding condition, the metals are tightly bonded, and no obvious gap is seen.

[0114] See also Figure 5 The figure shows the gap condition between the steel layer and the aluminum layer of the steel-aluminum composite fin tube manufactured by the traditional sleeve extrusion production process under a 50x microscope. It can be seen that there is an obvious gap between the steel layer and the aluminum layer, and this gap poses a risk of corrosion.

[0115] See also Figure 4 The 100x microscope observation shown shows the working condition of the interface area between the steel layer and the aluminum layer of the steel-aluminum composite fin tube manufactured by the production process of the present invention after the corrosion test. It can be seen that after the corrosion test, only the outer surface is corroded, and the interface area between the steel layer and the aluminum layer is not corroded. The steel layer and the aluminum layer have been combined into an integral, seamless one-piece structure, and there is no risk of corrosion in the interface area between the steel layer and the aluminum layer.

[0116] See also Figure 6 The figure shows the condition of the steel layer and aluminum layer interface area of ​​the steel-aluminum composite fin tube manufactured by the traditional sleeve extrusion production process after the corrosion test using a 100x microscope. It can be seen that after the corrosion test, corrosion occurs on the outer surface, corrosion occurs on the interface area between the copper layer and the aluminum layer, and there is an obvious gap in the interface area between the copper layer and the aluminum layer.

[0117] The manufacturing process of the composite finned tube disclosed in the present invention firstly casts the outer metal of the finned tube and the inner base tube 1 of the finned tube into an integrated composite tube 6 through a composite continuous casting process, so as to realize the continuous production of the long size of the composite tube 6, and then rolls the coated alloy layer material of the composite tube 6 into a plurality of fins through a fin rolling mill, so as to form a composite finned tube; finally, the surface of the steel-aluminum composite finned tube is subjected to a micro-arc oxidation reaction through a micro-arc oxidation device, so that a ceramic oxide film is formed on the surface of the steel-aluminum composite finned tube; the manufacturing process of the composite finned tube has low overall production cost and high processing production efficiency, and the base tube 1 of the produced composite finned tube is tightly combined with the outer metal material coated on the outside without gaps, thereby improving the strength and pressure bearing capacity of the composite finned tube, maintaining the overall rigidity of the component, and preventing deflection and deformation, avoiding damage to the base tube 1 due to erosion by air and fluid, and increasing the service life of the composite finned tube; the composite finned tube produced by the manufacturing process also has high hardness, excellent wear resistance, excellent corrosion resistance and excellent thermal stability.

[0118] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A manufacturing process for a composite finned tube, characterized in that: The process comprises a pipe continuous casting device, which comprises a casting furnace, a continuous casting mold is arranged in the casting furnace, the continuous casting mold extends to the outside of the casting furnace and is provided with a cooling crystallizer, a feeding device for conveying a base pipe and passing it through the continuous casting mold is arranged outside the casting furnace, and a traction device is arranged outside the casting furnace at the discharge of the continuous casting mold; an outer layer of metal melt for coating the outer wall of the base pipe is contained in the casting furnace; The process includes the following steps: S1. Insert the base tube into the continuous casting mold of the casting furnace, and there is a certain distance between the circumferential outer wall of the base tube and the molding cavity in the continuous casting mold. The outer layer of molten metal in the casting furnace flows into the molding cavity of the continuous casting mold and covers the base tube. The outer layer of molten metal in the continuous casting mold is cooled and solidified by a cooling crystallizer and attached to the base tube, thereby obtaining a composite tube; the base tube is continuously conveyed into the continuous casting mold by a feeding device, and the composite tube is pulled by a pulling device, thereby realizing continuous casting of the composite tube; S2, cutting the composite pipe formed by continuous casting into a specified length; S3, rolling the outer layer of the composite tube coating metal material into a plurality of fins by a fin rolling mill, thereby forming a composite fin tube; S4, using a fin tube head-pulling machine to pull the ends of the composite fin tube, and removing the fins from both ends of the composite fin tube according to the required length; S5. Cleaning, degreasing and pickling the composite fin tube to remove dirt and oxide layer on the surface of the composite fin tube; S6. The composite fin tube is fixed in the electrolytic cell of the micro-arc oxidation device by a fixture, so that the composite fin tube is completely immersed in the electrolyte, and a high voltage pulse is applied to generate micro-arc discharge on the surface of the composite fin tube to induce an oxidation reaction, so that a ceramic oxide film is formed on the surface of the composite fin tube; S7. Clean and dry the composite fin tube to remove residual electrolyte on the surface.

2. The manufacturing process of a composite fin tube according to claim 1, characterized in that: The base tube is a steel tube, and the outer layer of molten metal is molten aluminum.

3. The manufacturing process of a composite fin tube according to claim 1, characterized in that: After step S1, the composite pipe may be rolled and then cold drawn to adjust its wall thickness and outer diameter.

4. The manufacturing process of a composite fin tube according to claim 1, characterized in that: The conveying speed of the feeding device for the substrate pipe is 100-1500 mm / min.

5. The manufacturing process of a composite fin tube according to claim 1, characterized in that: The end of the base pipe is connected to an inert gas filling pipe, and inert gas is continuously filled into the base pipe through the inert gas filling pipe during the continuous casting process of the composite pipe.

6. The manufacturing process of a composite fin tube according to claim 1, characterized in that: The electrolyte in step S6 includes 5-30 g / L of water-soluble phosphate, 5-30 g / L of water-soluble silicate, 1-10 g / L of alkali metal hydroxide, 5-30 g / L of citrate, and 1-20 g / L of borate, and the solvent is deionized water.

7. The manufacturing process of a composite fin tube according to claim 1, characterized in that: The power source used by the micro-arc oxidation device in step S6 is a DC pulse power supply with a current density of 5-15A / dm², a frequency of 500HZ, a duty cycle of 4%, a temperature controlled at 20-30°C, and a constant current micro-arc oxidation time of 10-30min under continuous stirring.

8. The manufacturing process of a composite fin tube according to claim 1, characterized in that: The tube continuous casting device also includes a melting furnace for melting the outer layer of the composite fin tube cladding metal material into the outer layer metal melt. The melting furnace is connected to the casting furnace through a connecting pipe, and a plug is also provided at the liquid outlet of the melting furnace.

9. The manufacturing process of a composite fin tube according to claim 1, characterized in that: The continuous casting mold is a hollow tubular structure, with a composite hole at the center of the bottom of the continuous casting mold. The diameter of the composite hole is larger than the hollow hole of the continuous casting mold. The top of the hollow hole of the continuous casting mold is a positioning hole, and the diameter of the positioning hole is adapted to the outer diameter of the base tube. A drainage hole connected to the composite hole is provided on the circumferential side wall of the continuous casting mold.